Manufacturing method of steel-shell large-cylinder high-magnification sodium-ion battery

By adopting the steel-shell large cylindrical high-rate sodium ion battery manufacturing method in battery manufacturing, the challenge of improving the rate performance of traditional batteries is solved, and high-performance and low-cost high-rate characteristics are achieved, meeting market demand.

CN119050493AInactive Publication Date: 2024-11-29ZHEJIANG HUNA ENERGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411013365.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional cylindrical batteries face challenges in improving rate performance and comprehensive performance, and are difficult to meet the growing market demand.

Method used

Using the steel shell large cylindrical high-ratio sodium ion battery manufacturing method, the positive and negative electrode slurry is prepared in proportion, the design of high-pore diaphragms and new current collecting discs with strong overcurrent capabilities, and the selection of a magnification electrolyte is combined with the steel shell and the cap. Design to achieve high magnification characteristics.

Benefits of technology

A steel shell large cylindrical high-rate sodium ion battery with high performance and high magnification characteristics is achieved. It has simple process and low cost and excellent battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050493A_ABST
    Figure CN119050493A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a steel-shell large-cylinder high-magnification sodium-ion battery. The manufacturing method comprises the following steps: preparing a sheet, assembling and detecting. The steel-shell large-cylinder high-magnification sodium-ion battery is prepared by preparing positive and negative electrode slurry according to a proportion, designing a coating process, selecting a magnification type electrolyte and a high-pore diaphragm, designing a novel positive and negative electrode current collecting disc with high flow capacity, a steel shell and a cap and adopting a linking mode, the process is simple in preparation and low in cost, and meanwhile, the high-performance high-magnification sodium-ion battery has the characteristics of high performance and high magnification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery equipment, and in particular to a method for manufacturing a steel shell large cylindrical high-rate sodium ion battery. Background Art

[0002] With the development of the new energy industry, the application scenarios of new energy batteries are becoming more and more extensive and have penetrated into various fields. In order to adapt to the application of the industry, different types of batteries coexist in different application fields. Cost, capacity, life, safety, environmental adaptability, model, rate, etc. are comprehensive evaluation indicators for batteries.

[0003] Cylindrical batteries are widely used in energy storage, power supply, electric vehicles and other fields due to their low production cost, high production efficiency, safety and good rate performance. However, traditional cylindrical batteries still face challenges in further improving rate performance and comprehensive performance. Therefore, the development of new high-rate cylindrical batteries to meet the growing market demand has become an important research direction in the field of new energy. Summary of the invention

[0004] The object of the present invention is to provide a method for manufacturing a steel shell large cylindrical high-rate sodium ion battery that solves the above-mentioned problems.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for manufacturing a steel shell large cylindrical high-rate sodium ion battery, characterized in that the steps include: the first step, respectively mixing the ingredients of the positive electrode and the ingredients of the negative electrode to form a positive electrode slurry and a negative electrode slurry, uniformly coating the positive electrode slurry on an aluminum foil, uniformly coating the negative electrode material on a copper foil, and drying and rolling after coating to cut into positive electrode sheets and negative electrode sheets; the ingredients of the positive electrode include a positive electrode main material, a binder, a conductive paste and a composite conductive agent, the content of the positive electrode main material is 94.0% to 95.0%, the content of the binder is 1.5% to 2.0%, the conductive paste is 1.0% to 1.5%, and the composite conductive agent is 2.0% to 2.5%, and the ingredients of the negative electrode include a negative electrode main material: a composite binder: a thickener, a conductive agent, and the content of the negative electrode main material is 94.0% to 95.0% , composite binder 2.5~3.0%, thickener 1.0%~1.4%, conductive agent 2.0%~3.0%; the second step, the positive electrode sheet, separator and negative electrode sheet are wound into a battery core, and the pole ears at both ends of the positive and negative electrodes of the core are squeezed into a plane; the positive electrode collector plate and the negative electrode collector plate are welded to the flattened end faces of the positive and negative electrodes of the core respectively; grooves are punched on the battery shell, the welded core is pushed into the battery shell, and penetration welding is performed at the bottom of the battery to connect the internal and external circuits of the battery; the battery is baked to remove internal moisture and residual solvents, and the electrolyte is injected into the battery to seal the battery; the third step is to perform activation, formation and aging tests on the battery, and then sort it according to its capacity distribution, and perform various performance tests on the battery.

[0007] Preferably, the ingredient formula of the positive electrode is positive electrode main material: binder: conductive paste: composite conductive agent = 95.0%: 2.0%: 1.0%: 2.0%.

[0008] Preferably, the negative electrode ingredient formula is negative electrode main material: composite binder: thickener, conductive agent = 95.0%: 3.0%: 1.0%: 2.0%.

[0009] Preferably, the coating surface density of the positive electrode sheet is 1.25 to 1.45 g / 100 cm2.

[0010] Preferably, the coating area density of the negative electrode sheet is equal to the excess ratio, and the excess ratio = negative electrode capacity / positive electrode capacity = 1.15 to 1.20.

[0011] Preferably, the positive electrode current collector disk comprises a disk body, a current collector disk tab and a connector connecting the disk body and the current collector disk tab, and the current collector disk tab is laser welded to the cap; the negative electrode current collector disk is laser penetration welded to the battery casing, and the welding line is an open circle.

[0012] Preferably, the conductivity of the electrolyte is 8.0 mS / cm to 8.5 mS / cm; and the porosity of the diaphragm is 42%±2%.

[0013] Preferably, the thickness of the disk body and the thickness of the collector disk pole ear are both smaller than the thickness of the connector, the width of the disk body is larger than the width of the collector disk pole ear, and the width of the collector disk pole ear is larger than the width of the connector.

[0014] Preferably, the thickness of the bottom of the battery housing is greater than the wall thickness of the battery housing, and the wall thickness of the battery housing is greater than or equal to 0.5 mm.

[0015] The beneficial effects of the present invention are as follows: the present invention prepares positive and negative electrode slurries in proportion, designs coating processes, selects rate-type electrolytes, high-porous diaphragms, designs new positive and negative electrode current collecting plates, steel shells, caps and connection methods with strong current flow capacity to prepare large cylindrical steel shell high-rate sodium ion batteries. The process preparation is simple, the cost is low, and the battery has high performance and high-rate characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the process flow of the present invention;

[0017] Figure 2 It is a schematic structural diagram of the positive electrode current collecting disk of the present invention;

[0018] Figure 3 It is a schematic structural diagram of the cap of the present invention;

[0019] Figure 4 yes Figure 3 A schematic cross-sectional structure diagram of ;

[0020] Among them, there are a disc body 1, a current collecting disc ear 2, a connector 3, a through hole 4, a positive current collecting disc 5, a cap 6, an upper cover 7, an explosion-proof disc 8, a groove 9, an opening valve 10, and a sealing ring 11. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0022] In the description of the present invention, it should be noted that the terms "inside", "outside", "up", "down", "horizontal", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the present invention.

[0023] like Figures 1 to 4As shown, the present invention provides a method for manufacturing a large cylindrical steel shell high-rate sodium ion battery, the steps of which include: the first step, sheeting: the ingredients of the positive electrode and the ingredients of the negative electrode are mixed to form a positive electrode slurry and a negative electrode slurry, wherein the ingredients of the positive electrode include a positive electrode main material, a binder, a conductive slurry and a composite conductive agent, the positive electrode main material content is 94.0% to 95.0%, the binder content is 1.5% to 2.0%, the conductive slurry is 1.0% to 1.5%, and the composite conductive agent is 2.0% to 2.5%. The combination of conductive materials forms a tightly linked conductive network, which provides a prerequisite for the rapid embedding and extraction of ions. Furthermore, the composite conductive agent includes SP and KS6, and SP and KS6 each account for half of the composite conductive agent. The ingredients of the negative electrode include the main material of the negative electrode: a composite binder: a thickener, a conductive agent, the content of the main material of the negative electrode is 94.0% to 95.0%, the composite binder is 2.5 to 3.0%, the thickener is 1.0% to 1.4%, and the conductive agent is 2.0% to 3.0%. The negative electrode material itself has excellent conductivity, and with the composite binder, it is beneficial to maintain the stable structure of the pole piece and improve the battery rate and cycle performance during the rapid insertion and extraction of ions. Furthermore, the composite binder includes SBR and an aqueous binder, and SBR and the aqueous binder each account for half of the composite binder. The preferred positive electrode ingredient formula of the present invention is the main material of the positive electrode: binder: conductive slurry: composite conductive agent = 95.0%: 2.0%: 1.0%: 2.0%; the negative electrode ingredient formula is the main material of the negative electrode: composite binder: thickener, conductive agent = 95.0%: 3.0%: 1.0%: 2.0%. The positive electrode slurry is evenly coated on the aluminum foil, and the negative electrode material is evenly coated on the copper foil. During the coating process, the coating roller speed, gap and other parameters need to be controlled to ensure coating uniformity. After coating, it needs to be baked and dried, and then rolled and cut into positive and negative electrode sheets.

[0024] The second step is to wind the positive electrode sheet, separator and negative electrode sheet into a battery core, squeeze the tabs at both ends of the core into a flat surface; weld the positive collector plate and negative collector plate to the flattened end faces of the positive and negative electrodes of the core respectively; punch a groove on the battery shell, push the welded core into the battery shell, and perform penetration welding at the bottom of the battery to connect the internal and external circuits of the battery. The battery is baked to remove internal moisture and residual solvents, and the battery is sealed after injecting electrolyte into the battery.

[0025] The third step is to conduct activation, formation and aging tests on the batteries, then sort them according to their capacity distribution, and test various battery properties such as voltage.

[0026] Furthermore, the coating surface density of the positive electrode sheet is 1.25 to 1.45 g / 100 cm 2, which can meet the high rate requirements. To meet the high rate requirements. The coating surface density of the negative electrode sheet is obtained by the excess ratio, excess ratio = negative electrode capacity / positive electrode capacity = 1.15 ~ 1.20.

[0027] Furthermore, the positive electrode current collector 5 includes a disc body 1 for laser welding with a winding core (not shown), and a current collector tab 2 for welding with a cap. A foldable connector 3 for direct flow is provided between the disc body 1 and the current collector tab 2. The connector 3 is integrally connected to the disc body 1 and the current collector tab 2. Among them, a plurality of through holes 4 are provided on the disc body 1 to inject electrolyte and reduce the weight of the disc body 1. The thickness of the disc body 1 and the current collector tab 2 are both less than the thickness of the connector 3. The disc body 1 and the current collector tab 2 are relatively thin, which is conducive to welding. The disc body 1 and the current collector tab 2 are surface laser welded and surface flow, and the thickness should not be too large to ensure the welding effect. The connector 3 is a channel connecting the cap and the winding core, and the thickness can be increased to ensure sufficient flow capacity. The width of the disc body 1 is greater than the width of the collector plate lug 2, and the width of the collector plate lug 2 is greater than the width of the connector 3. The width of the disc body 1 and the collector plate lug 2 is increased to increase the area and ensure the current capacity. The thickness of the positive collector plate can be designed according to the current requirements, and the width can be designed according to the welding area of ​​the winding core and the cap. The negative collector plate and the battery case are laser-penetrated and welded, and the welding line is an open circle. The length and width of the welding line can be adjusted at any time to meet the current capacity requirements.

[0028] Furthermore, the conductivity of the electrolyte is 8.0mS / cm to 8.5mS / cm, which meets the rapid flow of sodium ions. The porosity of the diaphragm is 42%±2%. The cost of the above two materials is relatively low, but the impact is large, so design is preferred.

[0029] Furthermore, the present invention also includes a cap 6, including an upper cover 7 and an explosion-proof plate 8, and a groove 9 is provided on the explosion-proof plate 8 for wrapping the edge of the upper cover 7. A sealing ring 11 is provided on the periphery of the explosion-proof plate 8 for sealing. An opening valve 10 is provided on the upper cover 7, and the opening valve 10 is an unclosed circular notch, and the angle A at the opening of the circular notch is 60 degrees. When the internal pressure of the battery is too high, the opening valve 10 will open along its circular notch to release the internal pressure of the battery. The cap adopted by the present invention is a non-pull-off cap design, which eliminates the intermediate links and the current can be directly conducted to the outside.

[0030] Furthermore, the thickness of the bottom of the battery case is greater than the thickness of the side wall of the battery case, ensuring the negative electrode current flow, and the thickness of the side wall of the battery case is greater than or equal to 0.5 mm. The top thickness of the side wall of the battery case is greater than the bottom thickness of the side wall of the battery case, which not only enhances the stability of the battery case punching groove, but also ensures the sealing effect of the battery seal, effectively prevents the leakage of the electrolyte inside the battery, and improves the safety performance of the battery. The design of the variable wall structure of the side wall of the battery case effectively reduces the overall weight of the battery case, thereby improving the energy density of the battery.

[0031] The present invention prepares a steel shell large cylindrical high-rate sodium ion battery by preparing positive and negative electrode slurries in proportion, designing a coating process, selecting a rate-type electrolyte, a high-porous diaphragm, designing new positive and negative electrode current collecting plates with strong current flow capacity, a steel shell, a cap, and a connection method. The process preparation is simple, the cost is low, and it has high performance and high rate characteristics.

[0032] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0033] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for manufacturing a steel shell large cylindrical high-rate sodium ion battery, characterized in that: The steps include: first, mixing the positive electrode ingredients and the negative electrode ingredients to form positive electrode slurry and negative electrode slurry respectively, evenly coating the positive electrode slurry on aluminum foil, evenly coating the negative electrode material on copper foil, and drying and rolling and cutting into positive electrode sheets and negative electrode sheets after coating; the positive electrode ingredients include positive electrode main material, binder, conductive paste and composite conductive agent, the positive electrode main material content is 94.0% to 95.0%, the binder content is 1.5% to 2.0%, the conductive paste content is 1.0% to 1.5%, and the composite conductive agent content is 2.0% to 2.5%; the negative electrode ingredients include negative electrode main material: composite binder: thickener, conductive agent, negative electrode main material content is 94.0% to 95.0%, the composite binder content is 2.5% to 3.0 %, thickener 1.0%~1.4%, conductive agent 2.0%~3.0%; the second step, wind the positive electrode sheet, separator and negative electrode sheet into a battery core, and squeeze the pole ears at the positive and negative ends of the core into a plane; weld the positive electrode collector plate and the negative electrode collector plate to the flattened end faces of the positive and negative electrodes of the core respectively; punch grooves on the battery shell, push the welded core into the battery shell, and perform penetration welding at the bottom of the battery to connect the internal and external circuits of the battery; bake the battery to remove internal moisture and residual solvent, inject electrolyte into the battery and then seal the battery; the third step, perform activation, formation and aging tests on the battery, then sort it according to its capacity distribution, and perform various performance tests on the battery.

2. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The ingredient formula of the positive electrode is positive electrode main material: binder: conductive paste: composite conductive agent = 95.0%: 2.0%: 1.0%: 2.0%.

3. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The ingredient formula of the negative electrode is negative electrode main material: composite binder: thickener, conductive agent = 95.0%: 3.0%: 1.0%: 2.0%.

4. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The coating surface density of the positive electrode sheet is 1.25-1.45 g / 100 cm 2 .

5. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 4, characterized in that: The coating area density of the negative electrode sheet is equal to the excess ratio, and the excess ratio = negative electrode capacity / positive electrode capacity = 1.15 to 1.

20.

6. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The positive electrode current collector disk includes a disk body, a current collector disk tab and a connector connecting the disk body and the current collector disk tab, and the current collector disk tab is laser welded on the cap; the negative electrode current collector disk is laser penetrated and welded to the battery shell, and the welding line is an open circle.

7. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The conductivity of the electrolyte is 8.0 mS / cm to 8.5 mS / cm; the porosity of the diaphragm is 42%±2%.

8. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The thickness of the disk body and the thickness of the collector disk pole ear are both smaller than the thickness of the connector, the width of the disk body is larger than the width of the collector disk pole ear, and the width of the collector disk pole ear is larger than the width of the connector.

9. The method for manufacturing a steel shell large cylindrical high-rate sodium ion battery according to claim 1, characterized in that: The thickness of the bottom of the battery housing is greater than the wall thickness of the battery housing, and the wall thickness of the battery housing is greater than or equal to 0.5 mm.

Citation Information

Patent Citations

  • Preparation method for high-energy-density lithium ion battery

    CN109309232A

  • Method for manufacturing wound type sodium-ion battery

    CN110010843A

  • Preparation method of sodium battery

    CN117374406A