Full-silicon-wafer-size perovskite / crystalline silicon laminated solar cell and preparation method thereof

By setting a perovskite layer and slit coating process with different thicknesses in perovskite/silicon-based heterojunction stacked solar cells, the problem of short circuit risk in the packaging process of full-silicon wafer-sized batteries is solved, and the electrical performance is improved and conversion efficiency.

CN119053166AActive Publication Date: 2024-11-29LONGI GREEN ENERGY TECH CO LTD

Patent Information

Application Number
CN202411027488.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing full-silicon wafer-sized perovskite/silicon-based heterojunction stacked solar cells have a risk of short circuit during module packaging, mainly due to the increased direct contact between the window layer and the composite layer, which makes it difficult for electrical performance testing to meet future component requirements.

Method used

The perovskite layer is used to completely cover the silicon-based battery, and by setting the thickness difference between the central area and the peripheral area in the perovskite layer, ensuring that the thickness of the central area of ​​the perovskite layer is smaller than the thickness of the peripheral area, preventing the conduction between the composite layer and the window layer. At the same time, the perovskite layer is prepared using slit coating and other processes to reduce area damage and improve electrical performance.

Benefits of technology

It effectively reduces area damage caused by masks, improves the electrical performance of perovskite/crystalline silicon stacked solar cells in all silicon wafer sizes, reduces the risk of short circuits, and improves the stability and conversion efficiency of component processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004969629700000011
    Figure HDA0004969629700000011
  • Figure HDA0004969629700000021
    Figure HDA0004969629700000021
  • Figure HDA0004969629700000022
    Figure HDA0004969629700000022
Patent Text Reader

Abstract

The invention provides a full-silicon-wafer-size perovskite / crystalline silicon laminated solar cell and a preparation method thereof. Wherein the perovskite / crystalline silicon laminated solar cell comprises a silicon substrate cell and a perovskite cell which are sequentially laminated, and the perovskite cell comprises a perovskite layer. According to the full-silicon-wafer-size perovskite / crystalline silicon laminated solar cell, the thickness of the central region of the perovskite layer is smaller than that of the peripheral region, so that conduction of the composite layer and the window layer can be prevented, area damage caused by a mask is reduced, and the electrical performance of the full-silicon-wafer-size perovskite / crystalline silicon laminated solar cell is ensured. The front transparent conductive layer or the rear transparent conductive layer does not use a mask or has a small mask, the effective area is the same as the total area or has a small difference with the total area, and welding and packaging of a subsequent assembly process are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of solar cells, and specifically, relates to a full-silicon wafer-sized perovskite / crystalline silicon stacked solar cell and a preparation method thereof. Background Art

[0002] Organic-inorganic hybrid perovskite solar cells have attracted widespread attention worldwide as a new type of high-efficiency, low-cost solar cell. In just a few years, the photoelectric conversion efficiency of small-area single-junction perovskite cells has rapidly climbed from 3.8% in 2009 to more than 26%, and the photoelectric conversion efficiency of small-area perovskite / silicon heterojunction stacked cells has also reached more than 34%. The rapid efficiency development has made it the focus of current photovoltaic research institutions and companies. Compared with traditional thin-film solar cells (copper indium gallium selenide, cadmium telluride, etc.), perovskite solar cells have the advantages of high conversion efficiency, simple preparation process and low-cost potential, and have become the thin-film solar cell technology with the most industrial prospects. By adjusting the composition ratio of the precursor solution, the cutoff wavelength of the solar cell spectral response can be controlled, making it the most ideal top cell absorption layer material.

[0003] Silicon heterojunction solar cell technology has the advantages of simple process, low preparation temperature, high conversion efficiency, and symmetrical structure, and is considered to be the third generation of cell technology after PERC cells. Silicon heterojunction cells have high infrared band absorption, strong weak light effect, and structural advantages that can match pins, making them one of the best bottom cell choices. The "perovskite / silicon-based heterojunction" stacked cell structure is formed by perovskite cells (top cells) and silicon-based heterojunction cells (bottom cells) to achieve distributed absorption of the solar spectrum, which is expected to achieve higher conversion efficiency.

[0004] The current perovskite / silicon-based heterojunction stacked cells mainly focus on small-area devices. The substrate size is generally 2cm×2cm, and the effective area of ​​1cm×1cm in the center area is tested by masking. In perovskite / silicon-based heterojunction stacked cells, the window layer is generally a TCO material prepared by a PVD process. The perovskite top cell and the silicon-based heterojunction bottom cell are connected by a composite layer, which is also generally made of TCO material prepared by a PVD process. The window layer and the composite layer are isolated by a limited area and a perovskite layer in the middle to achieve an insulating effect. Due to the use of a mask, the area defined by the window layer and the composite layer only needs to be greater than or equal to the effective area, and does not need to reach the edge of the substrate.

[0005] However, with the development of technology, full-wafer-sized perovskite / silicon-based heterojunction stacked cells have become the main research object at present. Although the previous mask method to define the effective area can still meet the requirements of electrical performance testing, it can no longer meet the requirements of future component packaging. When packaging components, it is necessary to conduct electrical performance tests on the entire silicon wafer area without a mask on the perovskite / silicon-based heterojunction stacked cells. Therefore, on the full-wafer-sized perovskite / silicon-based heterojunction stacked cells, the effective area of ​​each film layer needs to be as close to the full silicon wafer size as possible. Since the window layer and the composite layer are both TCO materials prepared using the PVD process, the PVD process will have a certain amount of plating, which also greatly increases the probability of direct contact between the window layer and the composite layer, causing the full-wafer-sized perovskite / silicon-based heterojunction stacked cells to have the risk of short circuit. Summary of the invention

[0006] In view of the problems existing in the prior art, the present application provides a full silicon wafer-sized perovskite / crystalline silicon stacked solar cell and a preparation method thereof.

[0007] Specifically, this application involves the following aspects:

[0008] On the one hand, the present application provides a full silicon wafer-sized perovskite / crystalline silicon tandem solar cell, comprising a silicon substrate cell and a perovskite cell stacked in sequence, wherein the perovskite cell comprises a perovskite layer;

[0009] wherein the perovskite layer completely covers the silicon substrate cell;

[0010] The perovskite layer includes a central area and a peripheral area, wherein the central area refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area is less than the average thickness of the peripheral area.

[0011] Furthermore, the difference between the average thickness of the peripheral area and the average thickness of the central area is greater than or equal to 100 nm and less than or equal to 4000 nm, preferably greater than or equal to 200 nm and less than or equal to 2000 nm.

[0012] Furthermore, the peripheral area includes a first peripheral area and a second peripheral area, the first peripheral area refers to an area whose projection distance on the silicon substrate is greater than 1 mm and less than 2 mm from the edge of the silicon substrate battery, and the second peripheral area refers to an area whose projection distance on the silicon substrate is less than or equal to 1 mm from the edge of the silicon substrate battery;

[0013] The difference between the average thickness of the first peripheral region and the average thickness of the central region is greater than or equal to 100 nm and less than or equal to 2000 nm, preferably greater than or equal to 200 nm and less than or equal to 1000 nm;

[0014] The difference between the average thickness of the second peripheral region and the average thickness of the central region is greater than or equal to 200 nm and less than or equal to 4000 nm, preferably greater than or equal to 400 nm and less than or equal to 2000 nm.

[0015] Furthermore, the perovskite / crystalline silicon tandem solar cell also includes a composite layer, which is located between the silicon substrate cell and the perovskite cell, and the projection distance of the inner edge of the mask area of ​​the composite layer on the silicon substrate is less than or equal to 1 mm from the edge of the silicon substrate cell.

[0016] Furthermore, the perovskite cell includes a hole transport layer, a perovskite layer, an electron transport layer and a front transparent conductive layer which are stacked in sequence.

[0017] Furthermore, the distance between the projection of the inner edge of the mask region of the front transparent conductive layer on the silicon substrate and the edge of the silicon substrate battery is less than or equal to 1 mm.

[0018] Furthermore, the perovskite layer also extends toward the side of the perovskite / crystalline silicon tandem solar cell to cover at least a portion of the composite layer and the side of the silicon substrate cell.

[0019] Furthermore, the perovskite layer also extends toward the side of the perovskite / crystalline silicon tandem solar cell to cover at least a portion of the side of the hole transport layer.

[0020] Furthermore, the perovskite layer further extends to partially cover at least a portion of the back side of the silicon substrate cell.

[0021] Furthermore, the silicon substrate cell is a heterojunction cell, a tunneling oxide layer passivation contact cell, or a back contact cell.

[0022] Furthermore, the heterojunction cell includes an N-type amorphous silicon layer, a first intrinsic amorphous silicon layer, an N-type crystalline silicon substrate, a second intrinsic amorphous silicon layer, a P-type amorphous silicon layer and a rear transparent conductive layer which are stacked in sequence.

[0023] Furthermore, the distance between the projection of the inner edge of the mask region of the rear transparent conductive layer on the silicon substrate and the edge of the silicon substrate battery is less than or equal to 1 mm.

[0024] Furthermore, the N-type crystalline silicon substrate is a whole or half piece of M6, M10, or M12 silicon wafer.

[0025] On the other hand, the present application also provides a photovoltaic module, comprising any one of the above-mentioned perovskite / crystalline silicon tandem solar cells.

[0026] On the other hand, the present application also provides a method for preparing a full silicon wafer-sized perovskite / crystalline silicon tandem solar cell, comprising the following steps:

[0027] Preparation of silicon substrate cells;

[0028] forming a composite layer and a hole transport layer in sequence on the silicon substrate cell;

[0029] Preparing a perovskite layer on the hole transport layer so that the perovskite layer completely covers the silicon substrate cell;

[0030] sequentially preparing an electron transport layer and a front transparent conductive layer on the perovskite layer;

[0031] The perovskite layer includes a central area and a peripheral area, wherein the central area refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area is less than the average thickness of the peripheral area.

[0032] Furthermore, the distance between the projection of the mask region of the composite layer on the silicon substrate and the edge of the silicon substrate battery is less than or equal to 1 mm.

[0033] Furthermore, the distance between the projection of the mask region of the front transparent conductive layer on the silicon substrate and the edge of the silicon substrate battery is less than or equal to 1 mm.

[0034] Furthermore, the perovskite layer is prepared by slit coating, doctor blade coating, spray coating, inkjet printing, transfer printing or screen printing.

[0035] Furthermore, the perovskite / crystalline silicon tandem solar cell prepared by the preparation method is any one of the above-mentioned perovskite / crystalline silicon tandem solar cells.

[0036] The central area thickness of the perovskite layer in the full silicon wafer size perovskite / crystalline silicon stacked solar cell of the present application is less than the peripheral area thickness, which can prevent the conduction between the composite layer and the window layer, thereby reducing the area damage caused by the mask and ensuring the electrical performance of the full silicon wafer size perovskite / crystalline silicon stacked solar cell. The front transparent conductive layer or the rear transparent conductive layer of the present application does not use a mask or the mask is very small, and the effective area is the same as the total area or the difference is very small, which is helpful for the welding and packaging of the subsequent component process. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1A schematic diagram of a method for calculating the average thickness of a perovskite layer of a perovskite tandem cell with a velvet-structured bottom cell;

[0038] Figure 2 This is a schematic diagram of the structure of a perovskite / silicon-based heterojunction stacked battery in Comparative Example 1;

[0039] Figure 3 Schematic diagram of the structure of the perovskite / silicon-based heterojunction stacked battery of Comparative Example 2;

[0040] Figure 4 This is a schematic diagram of the structure of a perovskite / silicon-based heterojunction stacked battery in Example 1;

[0041] Figure 5 This is a schematic diagram of the structure of a perovskite / silicon-based heterojunction stacked battery in Example 2;

[0042] Figure 6 This is a schematic diagram of the structure of a perovskite / silicon-based heterojunction stacked battery in Example 3;

[0043] Figure 7 Schematic diagram of the structure of the perovskite layer surface of the perovskite tandem battery.

[0044] Reference numerals:

[0045] 1-1N-type crystalline silicon substrate, 1-2 first intrinsic amorphous silicon layer, 1-3P-type amorphous silicon layer, 1-4N-type amorphous silicon layer, 1-5 rear transparent conductive layer, 1-6 second intrinsic amorphous silicon layer, 2-1 composite layer, 3-1 hole transport layer, 3-2 perovskite layer, 3-3 electron transport layer, 3-4 front transparent conductive layer, 4-1 front metal electrode, 4-2 rear metal electrode, 6-1 central region, 6-2 first peripheral region, 6-3 second peripheral region. DETAILED DESCRIPTION

[0046] The present application is further described below in conjunction with examples. It should be understood that the examples are only used to further describe and illustrate the present application and are not used to limit the present application.

[0047] Unless otherwise defined, the technical and scientific terms in this specification have the same meaning as those generally understood by those skilled in the art. Although similar or identical methods and materials as described herein may be used in experiments or practical applications, materials and methods are described herein below. In the event of a conflict, the present specification including the definitions therein shall prevail. In addition, materials, methods and examples are provided for illustration only and are not restrictive. The present application is further described below in conjunction with specific embodiments, but is not intended to limit the scope of the present application.

[0048] In the present application, the average thickness is the average value of the thickness measured at any two or more test points in the corresponding area. When the average thickness of the perovskite layer is detected, for example, any two test points, three test points, four test points, five test points, six test points, seven test points, eight test points, nine test points, or more than ten test points can be randomly selected in the corresponding area of ​​the perovskite layer, such as the central area or the peripheral area, for detection and calculation. These test points can be at any position in the central area or the peripheral area, or they must be dispersed in an area of ​​a certain area, such as dispersed in 1mm 2 , 2mm 2 , 3mm 2 , 5mm 2 , 7mm 2 , 9mm 2 , 1cm 2 , 2cm 2 , 3cm 2 、4cm 2 , 5cm 2 、6cm 2 、7cm 2 、8cm 2 、9cm 2 、10cm 2 wait.

[0049] In the present application, the thickness of the perovskite layer can be detected by a thickness measurement method known in the art, for example, it can be measured by SEM.

[0050] In a specific embodiment, the silicon substrate cell has a velvet structure, and considering that the thickness of the perovskite layer is inconsistent at various locations. When testing the thickness of the perovskite layer, the thinnest position from the pyramid tip within the field of view to the upper surface of the perovskite layer is recorded as Tmin, and the thickest position from the pyramid bottom within the field of view to the upper surface of the perovskite layer is recorded as Tmax. The average thickness of the perovskite layer is (Tmin+Tmax) / 2. Figure 1 As shown in Figure A, Tmin is 566nm, Tmax is 1070nm, and the average thickness is 818nm. Figure 1 As shown in Figure B, Tmin is 770nm, Tmax is 1260nm, and the average thickness is 1015nm. Figure 1 As shown in Figure C, Tmin is 960nm, Tmax is 1600nm, and the average thickness is 1280nm.

[0051] Those skilled in the art will understand that, for the case where the silicon-based battery has a non-velvet structure, when detecting the average thickness of the perovskite layer, the average value of the thickness measured at any two or more of the above-mentioned test points can be selected, or the above-mentioned measurement method for the velvet structure can be adopted.

[0052] In the prior art, when preparing full-wafer-sized perovskite / silicon-based heterojunction stacked cells, the edge area is thin or incompletely covered, and conduction will occur between the composite layer and the window layer. To prevent conduction between the window layer and the composite layer, two implementation methods are generally used: one is to mask the window layer and the composite layer, and lose a certain power generation area. This method will reduce the effective power generation area and reduce the power generation efficiency of the full-wafer-sized perovskite / silicon-based heterojunction stacked cells; the other is not to mask the window layer and the composite layer, and after completing all the processes, the edges are cut. This method will damage the edge passivation layer of the bottom cell, resulting in serious leakage of the bottom cell, affecting the power generation efficiency of the full-wafer-sized perovskite / silicon-based heterojunction stacked cells. The second method sometimes performs special passivation or insulation treatment on the cut edges to reduce the conduction between the window layer and the composite layer, but the passivation effect needs further verification.

[0053] In view of these problems existing in the prior art, the present application provides a full silicon wafer-sized perovskite / crystalline silicon tandem solar cell. The full silicon wafer-sized perovskite / crystalline silicon tandem solar cell described in the present application refers to a cell in which the perovskite layer completely covers the silicon substrate.

[0054] like Figure 2-Figure 6 As shown, the perovskite / crystalline silicon tandem solar cell of the present application includes a silicon substrate cell and a perovskite cell stacked in sequence, wherein the perovskite cell includes a perovskite layer. Further, the perovskite / crystalline silicon tandem solar cell also includes a composite layer 2-1, and the composite layer 2-1 is located between the silicon substrate cell and the perovskite cell. The perovskite cell includes a hole transport layer 3-1, a perovskite layer 3-2, an electron transport layer 3-3, and a front transparent conductive layer 3-4 (i.e., the window layer mentioned in this article) stacked in sequence.

[0055] The perovskite layer 3-2 completely covers the silicon substrate battery. Those skilled in the art will appreciate that, generally, the composite layer 2-1 completely covers the silicon substrate battery, the hole transport layer 3-1 completely covers the composite layer 2-1, and the perovskite layer 3-2 completely covers the hole transport layer. Figure 7 As shown, the perovskite layer 3-2 includes a central area 6-1 and a peripheral area, wherein the central area 6-1 refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area 6-1 is less than the average thickness of the peripheral area.

[0056] The thickness of the central area of ​​the perovskite layer 3-2 is less than that of the peripheral area, which can prevent the conduction of the two conductive layers above and below the perovskite (such as the composite layer 2-1 and the window layer), thereby reducing the area damage caused by the mask and improving the overall conversion efficiency of the perovskite / crystalline silicon stacked solar cell.

[0057] In a specific embodiment, the difference between the average thickness of the peripheral area and the average thickness of the central area is greater than or equal to 100nm and less than or equal to 4000nm, for example, it can be 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, 2100nm, 2200nm, 2300nm, 2400nm, 2500nm, 2600nm, 2700nm, 2800nm, 2900nm, 3000nm, 3100nm, 3200nm, 3300nm, 3400nm, 3500nm, 3600nm, 3700nm, 3800nm, 3900nm, 4000nm, 4100nm, 4200nm, 4300nm, 4400nm, 4500nm, 4600nm, 4700nm, 4800nm, 4900nm, 5000nm, 5100nm, 5200nm, 5300nm, 5400nm, 5500nm, 5600nm, 5700nm, 5800nm, 5900nm, 600nm, 6100nm, 6100nm, 6200nm 800nm, 1900nm, 2000nm, 2100nm, 2200nm, 2300nm, 2400nm, 2500nm, 2600nm, 2700nm, 2800nm, 2900nm, 3000nm, 3100nm, 3200nm, 3300nm, 3400nm, 3500nm, 3600nm, 3700nm, 3800nm, 3900nm, 4000nm, and any value between these values.

[0058] In a specific embodiment, the difference between the average thickness of the peripheral region and the average thickness of the central region is greater than or equal to 200 nm and less than or equal to 2000 nm.

[0059] like Figure 7 As shown, further, from the perspective of reducing the difficulty of the preparation process, the peripheral area further includes a first peripheral area 6-2 and a second peripheral area 6-3, the first peripheral area 6-2 refers to an area whose projection distance on the silicon substrate is greater than 1 mm and less than 2 mm from the edge of the silicon substrate battery, and the second peripheral area 6-3 refers to an area whose projection distance on the silicon substrate is less than or equal to 1 mm from the edge of the silicon substrate battery.

[0060] In a specific embodiment, the difference between the average thickness of the first peripheral region 6-2 and the average thickness of the central region 6-1 is greater than or equal to 100nm and less than or equal to 2000nm, for example, it can be 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, and any value therebetween; the difference between the average thickness of the second peripheral region 6-3 and the average thickness of the central region 6-1 is greater than or equal to 200nm and less than or equal to 4000nm, for example, it can be 20 0nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, 2100nm, 2200nm, 2300nm, 2400nm, 2500nm, 2600nm, 2700nm, 2800nm, 2900nm, 3000nm, 3100nm, 3200nm, 3300nm, 3400nm, 3500nm, 3600nm, 3700nm, 3800nm, 3900nm, 4000nm, and any value between these values.

[0061] In a specific embodiment, the difference between the average thickness of the first peripheral region 6-2 and the average thickness of the central region 6-1 is greater than or equal to 200nm and less than or equal to 1000nm, and the difference between the average thickness of the second peripheral region 6-3 and the average thickness of the central region 6-1 is greater than or equal to 400nm and less than or equal to 2000nm.

[0062] Furthermore, if Figure 4 and Figure 5 As shown, the perovskite layer 3-2 can also extend to the side of the perovskite / crystalline silicon tandem solar cell to cover the hole transport layer 3-1, the composite layer 2-1 and at least a portion of the side of the silicon substrate cell.

[0063] like Figure 5 As shown, when the above extension degree is relatively high, the perovskite layer 3-2 can be further extended to partially cover at least a portion of the back side of the silicon substrate cell.

[0064] When the perovskite layer 3-2 forms a certain coverage on the edge and back of the stacked battery, it can simultaneously achieve the insulation effect between the window layer and the rear transparent conductive layer, thereby further reducing the risk of short circuit of the stacked battery and improving the stability of the preparation process.

[0065] In a specific embodiment, the distance between the projection of the inner edge of the mask area of ​​the front transparent conductive layer 3-4 on the silicon substrate and the edge of the silicon substrate battery, that is, the width of the mask area is less than or equal to 1 mm, for example, it can be 1 mm, 900nm, 800nm, 700nm, 600nm, 500nm, 400nm, 300nm, 200nm, 100nm, 50nm, 20nm, 10nm, 0, and any value in between.

[0066] In a specific embodiment, the distance between the projection of the inner edge of the mask area of ​​the composite layer 2-1 on the silicon substrate and the edge of the silicon substrate battery, that is, the width of the mask area is less than or equal to 1 mm, for example, it can be 1 mm, 900nm, 800nm, 700nm, 600nm, 500nm, 400nm, 300nm, 200nm, 100nm, 50nm, 20nm, 10nm, 0, and any value between these values.

[0067] The silicon-based cell of the present application may be any silicon-based cell suitable for perovskite stack cells in the art, such as a heterojunction cell, a tunneling oxide layer passivation contact cell, or a back contact cell.

[0068] In a specific embodiment, the silicon substrate cell is a heterojunction cell, such as Figure 2-6 As shown, it includes an N-type amorphous silicon layer 1-4, a first intrinsic amorphous silicon layer 1-2, an N-type crystalline silicon substrate 1-1, a second intrinsic amorphous silicon layer 1-6, a P-type amorphous silicon layer 1-3 and a rear transparent conductive layer 1-5 which are stacked in sequence.

[0069] The N-type crystalline silicon substrate may be of various models and sizes known in the art, such as a whole or half wafer of M6, M10, or M12 silicon wafer.

[0070] In a specific embodiment, the distance between the projection of the inner edge of the mask area of ​​the rear transparent conductive layer 1-5 on the silicon substrate and the edge of the silicon substrate battery, that is, the width of the mask area is less than or equal to 1 mm, for example, it can be 1 mm, 900nm, 800nm, 700nm, 600nm, 500nm, 400nm, 300nm, 200nm, 100nm, 50nm, 20nm, 10nm, 0, and any value in between.

[0071] The projection distance of the mask area of ​​the front transparent conductive layer 3-4, the composite layer 2-1, or the rear transparent conductive layer 1-5 on the silicon substrate is less than or equal to 1 mm from the edge of the silicon substrate battery, so that the effective area is the same as the total area or the difference is very small, which can reduce the impact on the power generation area. In addition, the front transparent conductive layer 2-1 or the rear transparent conductive layer 1-5 of the present application does not use a mask or the mask is very small, which is also helpful for the welding and packaging of the subsequent component process.

[0072] The materials and thicknesses of the composite layer 2-1, the hole transport layer 3-1, the electron transport layer 3-3 and the front transparent conductive layer 3-4 of the present application can adopt conventional materials and thicknesses in the art, and are not further limited here.

[0073] Specifically, the material of the hole transport layer is organic or inorganic. When it is organic, the hole transport layer is Spiro-TTB, Spiro-OMeTAD, Spiro-TAD, PTAA or PEDOT-PSS. When the hole transport layer is inorganic, the material of the hole transport layer is NiO x 、NiMgO x 、CoO、FeO、NiMgO x , V2O5, MoO3, Cr2O3 or compounds containing Cu(l).

[0074] The composite layer can realize the passage of photogenerated carriers from the perovskite layer to the silicon substrate battery, and is usually composed of TCO materials, such as one or more stacked layers of ITO, IWO, IZO, ITiO, AZO, GZO, FTO, IWO and graphene.

[0075] The materials of the electron transport layer are generally C60, PCBM, SnO2, etc.

[0076] The perovskite layer usually has a band gap of more than 1.6 eV. The material can be selected from a substance with an ABX3 structure, wherein A is selected from one or more of Cs, Rb, CH3NH3, HC(NH2)2, CH3(CH2)3NH3, (C6H5)(CH2)2NH3; B is selected from any one of Pb, Sn and Ge; X is a halogen. Preferably, A is a hybrid of inorganic and organic ions, such as (Cs 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 )3, etc.

[0077] Furthermore, a buffer layer may be provided between the perovskite layer 3-2 and the hole transport layer 3-1 to improve the conversion efficiency or stability of the battery.

[0078] An anti-reflection film layer may also be provided on the surface of the front transparent conductive layer 3-4 to improve the photoelectric conversion efficiency of the perovskite / silicon heterojunction stacked solar cell.

[0079] The present application also provides a photovoltaic module, comprising any one of the above-mentioned perovskite / crystalline silicon stacked solar cells.

[0080] The present application also provides a method for preparing a full silicon wafer-sized perovskite / crystalline silicon tandem solar cell, comprising the following steps:

[0081] Preparation of silicon substrate cells;

[0082] forming a composite layer and a hole transport layer in sequence on the silicon substrate cell;

[0083] Preparing a perovskite layer on the hole transport layer so that the perovskite layer completely covers the silicon substrate cell;

[0084] sequentially preparing an electron transport layer and a front transparent conductive layer on the perovskite layer;

[0085] The perovskite layer includes a central area and a peripheral area, wherein the central area refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area is less than the average thickness of the peripheral area.

[0086] The perovskite layer can be prepared by slit coating, doctor blade coating, spray coating, inkjet printing, transfer printing or screen printing, as long as the average thickness of the central area is less than the average thickness of the peripheral area.

[0087] In a specific embodiment, the perovskite layer is prepared by a slit coating method. The material utilization rate is about 95% using the slit coating process. On the one hand, it can reduce material waste and save material costs. On the other hand, it can reduce environmental pollution caused by the scrapping of the perovskite solution.

[0088] In a specific embodiment, when preparing the front transparent conductive layer, the projection distance of the mask region of the front transparent conductive layer on the silicon substrate is less than or equal to 1 mm from the edge of the silicon substrate battery.

[0089] In a specific embodiment, when preparing the composite layer, the distance between the projection of the mask region of the composite layer on the silicon substrate and the edge of the silicon substrate cell is less than or equal to 1 mm.

[0090] In a specific embodiment, the perovskite / crystalline silicon tandem solar cell prepared by the preparation method is any one of the above-mentioned perovskite / crystalline silicon tandem solar cells.

[0091] Example

[0092] Average thickness test method: Because silicon-based cells have a velvet structure, the thickness of the perovskite layer is inconsistent at various locations. When testing the thickness of the perovskite layer, the thinnest position from the pyramid tip within the field of view to the upper surface of the perovskite layer is recorded as Tmin, and the thickest position from the pyramid bottom within the field of view to the upper surface of the perovskite is recorded as Tmax. The average thickness of the perovskite layer is (Tmin+Tmax) / 2. The thickness is measured by SEM.

[0093] Comparative Example 1

[0094] Large-area perovskite / silicon-based heterojunction stacked cells with large-size masks for each TCO layer, such as Figure 2 As shown, the specific preparation method is as follows.

[0095] 1.1. Preparation of bottom battery.

[0096] 1.1.1, N-type crystalline silicon substrate 1-1

[0097] Commercial grade M10 size (182mm×182mm) N-type silicon wafers with a resistivity of 5Ω.cm and a thickness of 170μm were used. The silicon wafers were polished, textured and cleaned in sequence to obtain a small texture surface with a texture pyramid height of ≤2μm.

[0098] 1.1.2 Intrinsic amorphous silicon layer

[0099] PECVD is used to deposit 5 nm intrinsic amorphous silicon passivation layers on both sides of the silicon wafer to form front and back passivation layer films, namely, the first intrinsic amorphous silicon layer 1-2 and the second intrinsic amorphous silicon layer 1-6.

[0100] 1.1.3 N-type amorphous silicon layer 1-4

[0101] Phosphorus doping (doping concentration 10 19-20 cm -3 ) of 5nm N-type amorphous silicon layer constitutes the front field structure;

[0102] 1.1.4, P-type amorphous silicon layer 1-3

[0103] Boron doping (doping concentration 10) was deposited on the back of the silicon wafer by PECVD. 19-20 cm -3 )’s 5nm P-type amorphous silicon layer constitutes the back emitter structure.

[0104] 1.1.5, rear transparent conductive layer 1-5

[0105] The 120nm ITO layer is prepared by magnetron sputtering to collect photogenerated carriers and transfer them to the back metal electrode. A pre-designed mask is used to prepare the rear transparent conductive layer, so that the rear transparent conductive layer is patterned according to the design scheme, and the patterning size is 160mm×160mm.

[0106] 1.1.6, Composite layer 2-1

[0107] The 10nm ITO layer prepared by magnetron sputtering realizes the passage of photogenerated carriers from the perovskite layer to the silicon heterojunction. A pre-designed mask is used to prepare the composite layer, so that the composite layer is patterned according to the design scheme, and the patterning size is 160mm×160mm. The position of the composite layer is relatively symmetrical with the rear transparent conductive layer, that is, the center point of the composite layer projection position, the center point of the rear transparent conductive layer and the center point of the silicon wafer coincide, and the shapes of the composite layer, the rear transparent conductive layer and the silicon wafer are similar patterns.

[0108] 1.2. Top Cell Preparation

[0109] 1.2.1. Hole transport layer 3-1

[0110] Preparation of 30nm NiO by magnetron sputtering x layer as a hole transport layer.

[0111] 1.2.2, Perovskite layer 3-2

[0112] The band gap of the perovskite layer is generally around 1.65eV. 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 ) 3-component system, weigh appropriate materials according to the molar ratio, dissolve them in a mixed solution of DMF and DMSO, with a concentration of 1.5 M. Then use the spin coating process, set the speed to 1500 rpm, spin coating for 30 seconds, and then quickly vacuumize after coating. After taking out, place it on a hot plate at 100°C for annealing for 30 minutes to obtain the perovskite layer 3-2.

[0113] Due to the shear force and centrifugal force of spin coating, the battery prepared by this method has no thick edge effect, and the middle area is thicker and the edge area is thinner. According to SEM testing, the average thickness of the perovskite layer in the center area is 1500nm, the average thickness of the perovskite layer 2mm away from the edge is 700nm, and the average thickness of the perovskite layer 1mm away from the edge is 500nm.

[0114] 1.2.3 Electron transport layer 3-3

[0115] First, a 25nm C layer was prepared by evaporation. 60 , and then further used ALD at 105°C for 160 cycles to prepare 16nm TiO2 to achieve longitudinal transport of carriers.

[0116] 1.2.4, front transparent conductive layer 3-4

[0117] 100nm IZO is prepared by magnetron sputtering to form a front transparent conductive film and an anti-reflection film, so as to achieve lateral electron transport to the front metal electrode 4-1. A pre-designed mask is used when preparing the front transparent conductive layer, so that the rear transparent conductive layer is patterned according to the design scheme, and the patterning size is 160mm×160mm. The position of the composite layer is relatively symmetrical with the rear transparent conductive layer, that is, the center point of the composite layer projection position, the center point of the rear transparent conductive layer and the center point of the silicon wafer coincide, and the shapes of the composite layer, the rear transparent conductive layer and the silicon wafer are similar patterns.

[0118] 1.2.5, front metal electrode 4-1, rear metal electrode 4-2

[0119] By screen printing, silver grid lines with a height of 40 μm are printed on the upper and lower surfaces as the front metal electrode 4-1 and the rear metal electrode 4-2 respectively to collect current and form a complete perovskite / silicon heterojunction stacked solar cell.

[0120] 1.2.6. Add a surface anti-reflection film layer on the front transparent conductive layer and prepare 120nm SiN by electron beam evaporation x , in order to improve the photoelectric conversion efficiency of perovskite / silicon heterojunction tandem solar cells.

[0121] Comparative Example 2

[0122] The conventional spin coating method is used to prepare the perovskite layer, and each TCO layer has a small-size mask for large-area perovskite / silicon-based heterojunction stacked cells such as Figure 3 The specific preparation method is as follows.

[0123] 2.1. Preparation of bottom battery.

[0124] 2.1.1—2.1.4 are the same as 1.1.1—1.1.4.

[0125] 2.1.5, rear transparent conductive layer 1-5

[0126] The 120nm ITO layer is prepared by magnetron sputtering to collect photogenerated carriers and transfer them to the back metal electrode. A pre-designed mask is used to prepare the rear transparent conductive layer, so that the rear transparent conductive layer is patterned according to the design scheme, and the patterning size is 180mm×180mm.

[0127] 2.1.6 Composite layer 2-1

[0128] The 10nm ITO layer prepared by magnetron sputtering realizes the passage of photogenerated carriers from the perovskite layer to the silicon heterojunction. A pre-designed mask is used to prepare the composite layer, so that the composite layer is patterned according to the design scheme, and the patterning size is 180mm×180mm. The position of the composite layer is relatively symmetrical with the rear transparent conductive layer, that is, the center point of the composite layer projection position, the center point of the rear transparent conductive layer and the center point of the silicon wafer coincide, and the shapes of the composite layer, the rear transparent conductive layer and the silicon wafer are similar patterns.

[0129] 2.2. Preparation of top battery, same as 1.2.

[0130] 2.2.1—2.2.3 are the same as 1.1.1—1.2.3.

[0131] According to SEM testing, the average thickness of the perovskite layer in the central area is 1500nm, the average thickness of the perovskite layer 2mm away from the edge is 700nm, and the average thickness of the perovskite layer 1mm away from the edge is 500nm.

[0132] 2.2.4. Front transparent conductive layer 3-4

[0133] 100nm IZO is prepared by magnetron sputtering to form a front transparent conductive film and an anti-reflection film, so as to achieve lateral electron transport to the front metal electrode 4-1. When preparing the front transparent conductive layer, a pre-designed mask is used to make the rear transparent conductive layer patterned according to the design scheme, and the patterning size is 180mm×180mm. The position of the composite layer is relatively symmetrical with the rear transparent conductive layer, that is, the center point of the composite layer projection position, the center point of the rear transparent conductive layer and the center point of the silicon wafer coincide, and the shapes of the composite layer, the rear transparent conductive layer and the silicon wafer are similar patterns.

[0134] 2.2.5. Same as 1.2.5.

[0135] 2.2.6. Same as 1.2.6.

[0136] Example 1

[0137] Large-area perovskite / silicon-based heterojunction stacked cells such as Figure 4 As shown in Figure 1, the perovskite layer has thick edges and is prepared as follows.

[0138] 3.1. Preparation of bottom battery.

[0139] 3.1.1—3.1.4 are the same as 1.1.1—1.1.4.

[0140] 3.1.5, Rear transparent conductive layer 1-5

[0141] The 120nm ITO layer is prepared by magnetron sputtering to collect photogenerated carriers and transmit them to the back metal electrode. A pre-designed mask is used to prepare the rear transparent conductive layer, so that the rear transparent conductive layer is patterned according to the design scheme, and the patterned rear transparent conductive layer is ≤0.5mm away from the edge of the silicon wafer substrate.

[0142] 3.1.6 Composite layer 2-1

[0143] The 10nm ITO layer prepared by magnetron sputtering enables the photogenerated carriers to pass from the perovskite layer to the silicon heterojunction. When preparing the composite layer, a pre-designed mask is used to make the composite layer patterned according to the design scheme, and the outermost edge of the patterned composite layer is ≤0.5mm away from the edge of the silicon wafer substrate.

[0144] 3.2. Top Cell Preparation

[0145] 3.2.1. Same as 1.2.1.

[0146] 3.2.2. Perovskite layer 3-2.

[0147] Perovskite layer selection (Cs 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 )3-component system, weigh appropriate materials according to the molar ratio, and dissolve them in a mixed solution of DMF and DMSO with a concentration of 1.0M. Then use a slit coating process, and the coating width of the slit coating blade is 180mm, which is slightly smaller than the full silicon wafer size of 182mm. Set the liquid inlet speed to 15μL / s, the blade travel speed to 12mm / s, and the perovskite precursor to be coated on the bottom battery, and then perform a rapid vacuum treatment. After taking it out, anneal it on a 100℃ hot stage for 30 minutes to obtain a perovskite layer. Among them, when performing a rapid vacuum treatment, through the design of the gas field (evacuating air from the bottom or all around to ensure that the gas above the perovskite layer flows from the center to the surroundings), the solvent in the edge area of ​​the perovskite liquid film can have a greater volatilization rate, so that the perovskite thickness at the edge is greater than the perovskite thickness in the center area.

[0148] According to SEM testing, the average thickness of the perovskite layer in the central area greater than 2 mm from the edge is 700 nm, the average thickness of the perovskite layer in the first peripheral area greater than 1 mm and less than 2 mm from the edge is 900 nm, and the average thickness of the perovskite layer in the second peripheral area less than or equal to 1 mm from the edge is 1500 nm.

[0149] 3.2.3: Same as 1.2.3.

[0150] 3.2.4. Front transparent conductive layer 3-4

[0151] 100nm IZO is prepared by magnetron sputtering to form a front transparent conductive film and an anti-reflection film, so as to achieve lateral electron transport to the front metal electrode 4-1. When preparing the front transparent conductive layer, a pre-designed mask is used to pattern the rear transparent conductive layer according to the design scheme, and the outermost edge of the patterned front transparent conductive layer is ≤0.5mm from the edge of the silicon wafer substrate.

[0152] 3.2.5. Same as 1.2.5.

[0153] 3.2.6. Same as 1.2.6.

[0154] Example 2

[0155] Large-area perovskite / silicon-based heterojunction stacked cells such as Figure 5 The perovskite layer covers the edge region, and the specific preparation method is as follows.

[0156] 4.1. Preparation of bottom battery. Same as 3.1

[0157] 4.2. Preparation of top battery.

[0158] 4.2.1. Same as 1.2.1.

[0159] 4.2.2 Perovskite layer 3-2

[0160] Perovskite layer selection (Cs 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 ) 3-component system, weigh appropriate materials according to the molar ratio, and dissolve them in a mixed solution of DMF and DMSO with a concentration of 1.0M. Then use a slit coating process, and the coating width of the slit coating blade is 182mm, which is the same as the 182mm size of the full silicon wafer. Set the liquid inlet speed to 15μL / s, the blade travel speed to 11mm / s, and the perovskite precursor to be coated on the bottom battery, and then perform a rapid vacuum treatment. After taking it out, anneal it on a 100℃ hot stage for 30min to obtain a perovskite layer. Among them, during the rapid vacuum treatment, through the design of the gas field (pumping air from the bottom or all around to ensure that the gas above the perovskite layer flows from the center to the surroundings), the solvent in the edge area of ​​the perovskite liquid film can have a greater volatilization rate, so that the perovskite thickness at the edge is greater than the perovskite thickness in the center area. At this time, its edge area is thicker than the middle area, and the perovskite layer covers the edge area.

[0161] According to SEM testing, the average thickness of the perovskite layer in the central area greater than 2 mm from the edge is 700 nm, the average thickness of the perovskite layer in the first peripheral area greater than 1 mm and less than 2 mm from the edge is 900 nm, the average thickness of the perovskite layer in the second peripheral area less than or equal to 1 mm from the edge is 1200 nm, and the average thickness of the side perovskite layer is 500 nm.

[0162] 4.2.3—4.2.6. Same as 3.2.3—3.2.6.

[0163] Example 3

[0164] Large-area perovskite / silicon-based heterojunction stacked cells such as Figure 6 As shown, the perovskite layer covers the edge area, and a small part is coated around the back of the silicon wafer. The specific preparation method is as follows.

[0165] 5.1. Preparation of bottom battery. Same as 3.1

[0166] 5.2. Preparation of top battery.

[0167] 5.2.1. Same as 1.2.1.

[0168] 5.2.2 Perovskite layer 3-2

[0169] Perovskite layer selection (Cs 0.15 FA 0.85 )Pb(I 0.7 Br 0.3 ) 3-component system, weigh appropriate materials according to the molar ratio, and dissolve them in a mixed solution of DMF and DMSO with a concentration of 1.0M. Then use a slit coating process, and the coating width of the slit coating blade is 184mm, which is slightly larger than the 182mm size of the full silicon wafer. Set the liquid inlet speed to 15μL / s, the blade travel speed to 10mm / s, and the perovskite precursor is coated on the bottom battery, and then a rapid vacuum treatment is performed. After taking it out, it is placed on a 100℃ hot stage for annealing for 30min to obtain a perovskite layer. Among them, when performing a rapid vacuum treatment, through the design of the gas field (air is pumped from the bottom or all around to ensure that the gas above the perovskite layer flows from the center to the surroundings), the solvent in the edge area of ​​the perovskite liquid film can have a greater volatilization rate, so that the perovskite thickness at the edge is greater than the perovskite thickness in the center area. At this time, its edge area is thicker than the middle area, and the perovskite layer bypasses the edge area, and partially covers the rear transparent conductive layer 1-5, and the coated area is ≤1mm away from the edge.

[0170] According to SEM testing, the average thickness of the perovskite layer in the central area greater than 2 mm from the edge is 700 nm, the average thickness of the perovskite layer in the first peripheral area greater than 1 mm and less than 2 mm from the edge is 800 nm, the average thickness of the perovskite layer in the second peripheral area less than or equal to 1 mm from the edge is 1000 nm, the average thickness of the side perovskite layer is 500 nm, and the average thickness of the perovskite layer in the local coating area of ​​the rear transparent conductive layer 1-5 is 1000 nm.

[0171] 4.2.3—4.2.6. Same as 3.2.3—3.2.6.

[0172] The electrical properties of the laminated solar cells prepared in Examples 1-3 and Comparative Examples 1-2 were measured. The measurement results are shown in Table 1.

[0173] Table 1

[0174] Electrical performance parameters Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Isc(A) 4.941 6.233 6.393 6.413 6.373 Voc(V) 1.99 1.72 1.99 1.98 1.99 FF(%) 81.03 67.31 79.56 79.67 79.61 Pmax(W) 7.967 7.216 10.121 10.116 10.096 <![CDATA[Effective area (cm 2 )]]> 256 324 331.23 331.23 331.23 <![CDATA[Eff 有效 (%)]]> 31.12 22.27 30.56 30.54 30.48 <![CDATA[Total area (cm 2 )]]> 331.23 331.23 331.23 331.23 331.23 <![CDATA[Eff 总 (%)]]> 24.05 21.78 30.56 30.54 30.48

[0175] As can be seen from Table 1, if only the effective area is considered, the masked TCO layer can achieve insulation between the composite layer and the window layer, and the stacked cell also has a high conversion efficiency. However, considering the total area, the masked perovskite / silicon-based heterojunction stacked cell has no conversion efficiency advantage. If a conventional spin coating process is used to prepare a large-area perovskite / silicon-based heterojunction stacked cell, the perovskite in the edge area is too thin and cannot even guarantee complete coverage, making it difficult to achieve complete insulation between the composite layer and the window layer, resulting in serious leakage. In the case of no TCO mask, the conversion efficiency of the full-wafer-sized perovskite / silicon-based heterojunction stacked cell is greatly affected.

[0176] With the full silicon wafer-sized perovskite / silicon-based heterojunction stacked cell of the present application, the composite layer and the window layer can be completely insulated, and whether each TCO layer uses a mask has little effect on the conversion efficiency of the effective area. The full silicon wafer-sized perovskite / silicon-based heterojunction stacked cell prepared in this way minimizes the mask area of ​​the window layer, thereby increasing the effective area of ​​the stacked cell and improving the overall conversion efficiency of the cell, having the conversion efficiency advantage of the entire silicon wafer area.

[0177] In addition, since the perovskite layer has a relatively thick thickness in the peripheral area and even forms a certain coverage on the edge and the back (Example 2 and Example 3), the insulation effect between the window layer TCO layer and the rear transparent conductive layer can be achieved at the same time, thereby further reducing the risk of short circuit of the stacked battery and improving the stability of the preparation process.

Claims

1. A full silicon wafer-sized perovskite / crystalline silicon tandem solar cell, comprising a silicon substrate cell and a perovskite cell stacked in sequence, wherein the perovskite cell comprises a perovskite layer; wherein the perovskite layer completely covers the silicon substrate cell; The perovskite layer includes a central area and a peripheral area, wherein the central area refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area is less than the average thickness of the peripheral area.

2. The perovskite / crystalline silicon tandem solar cell according to claim 1, wherein the difference between the average thickness of the peripheral region and the average thickness of the central region is greater than or equal to 100 nm and less than or equal to 4000 nm, preferably greater than or equal to 200 nm and less than or equal to 2000 nm.

3. The perovskite / crystalline silicon tandem solar cell according to claim 1 or 2, wherein the peripheral area comprises a first peripheral area and a second peripheral area, the first peripheral area refers to an area whose projection distance on the silicon substrate from the edge of the silicon substrate cell is greater than 1 mm and less than 2 mm, and the second peripheral area refers to an area whose projection distance on the silicon substrate from the edge of the silicon substrate cell is less than or equal to 1 mm; The difference between the average thickness of the first peripheral region and the average thickness of the central region is greater than or equal to 100 nm and less than or equal to 2000 nm, preferably greater than or equal to 200 nm and less than or equal to 1000 nm; The difference between the average thickness of the second peripheral region and the average thickness of the central region is greater than or equal to 200 nm and less than or equal to 4000 nm, preferably greater than or equal to 400 nm and less than or equal to 2000 nm.

4. The perovskite / crystalline silicon tandem solar cell according to any one of claims 1-3, wherein the perovskite / crystalline silicon tandem solar cell further comprises a composite layer, wherein the composite layer is located between the silicon substrate cell and the perovskite cell, and a projection distance of an inner edge of a mask region of the composite layer on the silicon substrate from an edge of the silicon substrate cell is less than or equal to 1 mm.

5. The perovskite / crystalline silicon tandem solar cell according to any one of claims 1 to 4, wherein the perovskite cell comprises a hole transport layer, a perovskite layer, an electron transport layer and a front transparent conductive layer stacked in sequence.

6. The perovskite / crystalline silicon tandem solar cell according to claim 5, wherein the projection distance of the inner edge of the mask area of ​​the front transparent conductive layer on the silicon substrate to the edge of the silicon substrate cell is less than or equal to 1 mm.

7. The perovskite / crystalline silicon tandem solar cell according to claim 4, wherein the perovskite layer also extends to the side of the perovskite / crystalline silicon tandem solar cell to cover at least a portion of the composite layer and the side of the silicon base cell.

8. The perovskite / crystalline silicon tandem solar cell according to claim 5, wherein the perovskite layer further extends toward the side of the perovskite / crystalline silicon tandem solar cell to cover at least a portion of the side of the hole transport layer.

9. The perovskite / crystalline silicon tandem solar cell according to claim 7, wherein the perovskite layer further extends to partially cover at least a portion of the back side of the silicon substrate cell.

10. The perovskite / crystalline silicon tandem solar cell according to any one of claims 1 to 9, wherein the silicon substrate cell is a heterojunction cell, a tunneling oxide layer passivation contact cell, or a back contact cell.

11. The perovskite / crystalline silicon tandem solar cell according to claim 10, wherein the heterojunction cell comprises an N-type amorphous silicon layer, a first intrinsic amorphous silicon layer, an N-type crystalline silicon substrate, a second intrinsic amorphous silicon layer, a P-type amorphous silicon layer and a rear transparent conductive layer stacked in sequence.

12. The perovskite / crystalline silicon tandem solar cell according to claim 11, wherein the projection distance of the inner edge of the mask area of ​​the rear transparent conductive layer on the silicon substrate to the edge of the silicon substrate cell is less than or equal to 1 mm.

13. The perovskite / crystalline silicon tandem solar cell according to any one of claims 1 to 12, wherein the N-type crystalline silicon substrate is a whole or half piece of M6, M10, or M12 silicon wafer.

14. A photovoltaic module, comprising the perovskite / crystalline silicon tandem solar cell according to any one of claims 1 to 13.

15. A method for preparing a full silicon wafer-sized perovskite / crystalline silicon tandem solar cell, comprising the following steps: Preparation of silicon substrate cells; forming a composite layer and a hole transport layer in sequence on the silicon substrate cell; Preparing a perovskite layer on the hole transport layer so that the perovskite layer completely covers the silicon substrate cell; sequentially preparing an electron transport layer and a front transparent conductive layer on the perovskite layer; The perovskite layer includes a central area and a peripheral area, wherein the central area refers to an area whose projection distance on the silicon substrate is greater than or equal to 2 mm from the edge of the silicon substrate battery, and the peripheral area refers to an area whose projection distance on the silicon substrate is less than 2 mm from the edge of the silicon substrate battery, wherein the average thickness of the central area is less than the average thickness of the peripheral area. 16 . The preparation method according to claim 15 , wherein the distance between the projection of the mask region of the composite layer on the silicon substrate and the edge of the silicon substrate cell is less than or equal to 1 mm. 17 . The preparation method according to claim 15 or 16 , wherein the distance between the projection of the mask region of the front transparent conductive layer on the silicon substrate and the edge of the silicon substrate battery is less than or equal to 1 mm.

18. The preparation method according to any one of claims 15 to 17, wherein the perovskite layer is prepared by slit coating, doctor blade coating, spray coating, inkjet printing, transfer printing or screen printing.

19. The preparation method according to any one of claims 15 to 18, wherein the perovskite / crystalline silicon tandem solar cell prepared by the preparation method is the perovskite / crystalline silicon tandem solar cell according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Solar cell, preparation method thereof and solar cell module

    CN115117112A

  • Perovskite battery and forming method thereof

    CN117042553A

  • Perovskite battery

    CN117082876A

  • Preparation method of semitransparent high-efficiency perovskite / silicon laminated solar cell

    CN118215307A

Cited By

  • Solar cell and solar cell string

    WO2026197180A1