Preparation method of light-emitting device based on exciplex
Through the preparation method based on excitation composite, the problems of high manufacturing cost and low raw material utilization are solved, and the TADF-OLED with high efficiency and green emission is achieved, with high brightness and high external quantum yield, and the process is simple. Low time and low energy consumption.
Patent Information
- Application Number
- CN202411147571.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing TADF emitters have high manufacturing costs and complex synthesis processes. The traditional evaporation method leads to low utilization of raw materials, serious waste, and affects production efficiency and costs.
Using the preparation method based on excitation composite, the electron donor material PO-T2T and the electron acceptor material BCzPh dissolve in an inert gas atmosphere to form an efficient green emitted excitation composite. The nano film was prepared by spin coating by solvent method, combined with PEDOT:PSS/PVK layer and thermal evaporation deposit TPBi, LiF, and Al layers to form efficient TADF-OLED.
High luminescence intensity, photoluminescence quantum yield reached 53%, high brightness 117011cd m-2 and high external quantum yield 13.36%, and improved the spectral stability and material utilization of the device, reducing production costs and time.
Smart Images

Figure CN119053205A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of chemical technology, and in particular to a method for preparing a light-emitting device based on an excimer complex. Background Art
[0002] Thermally activated delayed fluorescence (TADF) light-emitting diodes, as a new generation of organic light-emitting diodes (OLEDs), have attracted widespread application in academia and industry. According to self-selected statistics, the electrons and holes injected into the OLED emission layer (EML) will cause recombination, and then produce singlet and triplet excitons in a ratio of 25%:75%. For traditional fluorescent emission OLEDs, only singlet excitons can be used, while OLEDs based on phosphorescent emission have high costs and unclear toxicity of precious metal resources. Relatively speaking, due to the small singlet-triplet energy difference (EST) of TADF emitters, triplet excitons can return to the singlet energy level through reverse gap crossing, and most of the emitter composition is metal-free organic molecules. Therefore, TADFOLED has the excellent characteristics of high exciton utilization, low cost, low toxicity and simple manufacturing process.
[0003] Many methods have been applied to develop TADF emitters, such as designing organic molecules with high intramolecular charge transfer properties to achieve a reduction in the singlet-triplet energy difference (EST). However, this has led to a sharp increase in the manufacturing cost of the emitter and increased the complexity of the synthesis process. In addition, most organic molecules rely on thermal evaporation to form a uniform and stable nano-thickness emission layer, which further reduces the utilization rate of raw materials because a large amount of raw materials are wasted in a bulky evaporation chamber instead of being deposited on a preset conductive substrate.
[0004] In order to avoid the above-mentioned technical problems, it is necessary to use existing materials to form a complex with TADF emission characteristics as an OLED emitter to solve the actual production needs, and the good solubility of most organic molecules in common organic solvents can be used to realize solvent-based parts, and large-area printing can be achieved using low-concentration spin coating solvents, further improving the utilization rate of raw materials, strictly controlling time and economic costs, and solving actual production problems. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a light-emitting device based on an exciplex.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a light-emitting device based on an exciplex comprises the following steps:
[0008] Step 1: Dissolve BCzPh and PO-T2T in chromatography grade dichloromethane in an inert gas atmosphere to obtain corresponding solutions;
[0009] Step 2: Pour the PO-T2T solution and the BCzPh solution into a container and stir them under an inert gas environment at room temperature to obtain an exciplex mixed solution;
[0010] Step 3: Preliminary preparation of BCzPh:PO-T2T exciplex light-emitting device;
[0011] The ITO conductive glass was carefully cleaned with soap, deionized water, ethanol, chloroform, acetone and isopropanol, and then treated with UV-ozone.
[0012] A PEDOT:PSS solution (Baytron PVP Al4083) is spin-coated on the treated ITO conductive glass through a filter head, followed by annealing; the ITO conductive glass is then transferred to a glove box filled with an inert gas, PVK dissolved in a chlorobenzene solution is spin-coated on the PEDOT:PSS film, followed by annealing to form a PEDOT:PSS / PVK layer, which is used as a hole injection layer and a hole transport layer;
[0013] Spin-coat the exciplex mixed solution prepared in step 2 onto the PEDOT:PSS / PVK layer as a light-emitting layer;
[0014] Step 4: Transfer the product obtained in step 3 into a vacuum chamber, and sequentially deposit TPBi, LiF and Al layers by thermal evaporation, wherein the TPBi layer serves as an electron transport layer and a hole blocking layer, and the LiF and Al layers serve as top electrodes; thus, a light-emitting device based on an exciplex is obtained.
[0015] Preferably, in step 2, the addition ratio of PO-T2T solution and BCzPh solution is 1:1.
[0016] Preferably, in step 2, the stirring time is 5 min under an inert gas environment at room temperature, and the stirring speed is 600-1000 r / min.
[0017] Preferably, in step 1, the concentration ratio of BCzPh to PO-T2T is 1:1, and the volume ratio is 1:1.
[0018] Preferably, the inert gas in steps 1-3 is nitrogen.
[0019] Preferably, in step 3, the rotation speed of spin coating PeDOT:PSS is 2000 r / min, the rotation speed of spin coating PVK is 2000 r / min, and the rotation speed of spin coating the exciplex solution on the PeDOT:PSS / PVK layer is 1500 r / min.
[0020] Preferably, in step 3, the annealing treatment of PeDOT:PSS is specifically: annealing at a temperature of 170°C for 30 minutes; the annealing treatment of PVK is specifically: annealing at a temperature of 150°C for 15 minutes.
[0021] The beneficial effects of the present invention are:
[0022] The present invention proposes a method for preparing a light-emitting device based on an exciplex. During the preparation process, an electron donor material PO-T2T and an electron acceptor material BCzPh are first used to prepare an efficient green emitting exciplex. The complex not only has high solubility in various organic solvents, but also has a high degree of steric hindrance, so that the nanofilm obtained by solvent spin coating has high luminous intensity and luminous uniformity, and the photoluminescence quantum yield (PLQY) reaches 53%. Furthermore, the complex is used as an emission layer to prepare a pure green light TADF-OLED with an electroluminescence (EL) wavelength of 511nm. The device has a wavelength of 117011cd m -2 The device has a high brightness and a high external quantum yield (EQE) of 13.36%. At the same time, the balanced carrier transport environment in the device greatly improves the spectral stability of the device.
[0023] The present invention provides a method for preparing a light-emitting device based on an exciplex, which is simple to operate, takes little time, consumes low energy, and has simple process requirements. The TADF exciplex prepared by the method has good film-forming properties, high photoluminescence quantum yield, high color purity, and good device stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is the molecular structure formula of the electron donor material PO-T2T and the electron acceptor material BCzPh;
[0025] Figure 2 The intrinsic photoluminescence spectra of the electron acceptor material BCzPh and the electron donor PO-T2T and the photoluminescence spectrum of the excited complex BCzPh:PO-T2T;
[0026] Figure 3 To adjust the film transient photoluminescence spectra (TRPL) and the corresponding photoluminescence lifetime for the total concentration of BCzPh and PO-T2T;
[0027] Figure 4The temperature-dependent transient photoluminescence spectrum of the optimized BCzPh:PO-T2T exciplex film;
[0028] Figure 5 Two-dimensional and three-dimensional atomic force microscopy images of the optimized BCzPh:PO-T2T exciplex film;
[0029] Figure 6 Scanning electron microscope images (SEM) of BCzPh:PO-T2T exciplex films at different concentrations;
[0030] Figure 7 The energy level structure diagram of TADF-OLED based on BCzPh:PO-T2T exciplex;
[0031] Figure 8 Electroluminescence spectrum (EL) of the optimized BCzPh:PO-T2T exciplex;
[0032] Fig. 9 Brightness-voltage-current density curve of TADF-OLED with optimized BCzPh:PO-T2T exciplex;
[0033] Fig.10 The external quantum efficiency (EQE), current power (CE), and power efficiency-brightness curve (PE) of TADF-OLED with optimized BCzPh:PO-T2T excimer complex. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0035] In one embodiment, a method for preparing a high-efficiency green-emitting BCzPh:PO-T2T exciplex using an electron donor PO-T2T and an electron acceptor BCzPh, and preparing a light-emitting device based on the prepared exciplex is provided, the method comprising the following steps:
[0036] 1) First, 5 mg of PO-T2T and 5 mg of BCzPh were dissolved in 1.0 ml of chromatographically pure dichloromethane solution, and ultrasonic treatment was performed under an inert gas atmosphere until the solid was dissolved to obtain a precursor solution.
[0037] 2) Secondly, 5 mg / ml PO-T2T solution and 5 mg / ml BCzPh solution were sealed with sealing glue, transferred to a stirring table and stirred vigorously for 10 minutes, and then transferred to an ultrasonic cleaning machine for ultrasonic treatment. The process lasted for five minutes, and then allowed to stand for five minutes to form a spin coating solution with stable composition and uniform distribution.
[0038] 3) Preparation of TADF-OLEDs of BCzPh:PO-T2T exciplexes;
[0039] The ITO conductive glass was carefully cleaned with soap, deionized water, ethanol, chloroform, acetone and isopropanol, and then treated with UV-ozone.
[0040] A PEDOT:PSS solution (Baytron PVP Al 4083) was spin-coated on the treated ITO glass through a filter head at a speed of 2000 r / min for 30 seconds, and then annealed at a temperature of 170°C for 30 minutes; then the substrate was transferred to a glove box filled with N2 gas, and PVK dissolved in a chlorobenzene solution was spin-coated on the PEDOT:PSS film at a speed of 3000 r / min for 50 seconds, and then annealed at a temperature of 100°C for 10 minutes to finally form a PEDOT:PSS / PVK layer, and the PEDOT:PSS / PVK layer was used as a hole injection layer and a hole transport layer;
[0041] 4) Spin-coat the BCzPh:PO-T2T solution prepared in step 2) on the PEDOT:PSS / PVK layer as a light-emitting layer;
[0042] 5) The product obtained in step 4 is finally transferred into a vacuum chamber, and TPBi, LiF and Al layers are sequentially deposited by thermal evaporation, wherein the TPBi layer serves as an electron transport layer and a hole blocking layer, and the LiF and Al layers serve as top electrodes; thereby obtaining a TADF-OLED based on a BCzPh:PO-T2T excimer complex.
[0043] like Figure 1 As shown in Figure 2, the electron acceptor properties of BCzPh and the electron donor properties of PO-T2T can be used to construct a donor-acceptor exciplex. Figure 2 As shown in the figure, the BCzPh:PO-T2T film shows a photoluminescence peak position that is completely different from that of the original material, indicating that a new energy level has been formed, that is, the two have generated an exciplex. Figure 3 As shown in the figure, changing the overall concentration of the electron donor acceptor material significantly changes the average photoluminescence lifetime. This is due to the surface defect state generated at low concentrations and the concentration quenching at high concentrations. The best concentration representing the long lifetime is 5.0 mg / ml. Figure 4As shown in Figure 1, the temperature-dependent photoluminescence lifetime of the exciplex shows that as the temperature decreases, the photoluminescence lifetime has a short-lived component that decreases sharply, and the average lifetime is significantly enhanced, which indicates the thermally activated delayed fluorescence properties of the exciplex. Figure 5 As shown in Figure 2, the surface morphology of the optimized BCzPh:PO-T2T film has high crystallinity and uniform size, and the excellent film uniformity further proves the feasibility of light-emitting diode manufacturing. Figure 6 As shown in Figure 2, the morphological characteristics of the film surface were further observed using scanning electron microscope images, further confirming the flatness of the film. Figure 7 As shown, an electroluminescent device was prepared using the BCzPh:PO-T2T excimer complex. The structure in the figure ensures the smooth transport of two types of carriers inside the device. Figure 8 The electroluminescence spectrum of the device is shown to have high chromaticity and stability. Fig. 9 As shown in Figure 10, the EQE, CE, and PE of the electroluminescent device all reach relatively high values in the field.
[0044] The present invention proposes a method for preparing a light-emitting device based on an exciplex. During the preparation process, an electron donor material PO-T2T and an electron acceptor material BCzPh are first used to prepare an efficient green emitting exciplex. The complex not only has high solubility in various organic solvents, but also has a high degree of steric hindrance, so that the nanofilm obtained by solvent spin coating has high luminous intensity and luminous uniformity, and the photoluminescence quantum yield (PLQY) reaches 53%. Furthermore, the complex is used as an emission layer to prepare a pure green light TADF-OLED with an electroluminescence (EL) wavelength of 511nm. The device has a wavelength of 117011cd m -2 The device has a high brightness and a high external quantum yield (EQE) of 13.36%. At the same time, the balanced carrier transport environment in the device greatly improves the spectral stability of the device.
[0045] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a light-emitting device based on an exciplex, characterized in that: The following steps are involved: Step 1: Dissolve BCzPh and PO-T2T in chromatography grade dichloromethane in an inert gas atmosphere to obtain corresponding solutions; Step 2: Pour the PO-T2T solution and the BCzPh solution into a container and stir them under an inert gas environment at room temperature to obtain an exciplex mixed solution; Step 3: Preliminary preparation of BCzPh:PO-T2T exciplex light-emitting device; The ITO conductive glass was carefully cleaned with soap, deionized water, ethanol, chloroform, acetone and isopropanol, and then treated with UV-ozone. A PEDOT:PSS solution is spin-coated on the treated ITO conductive glass through a filter head, followed by annealing; the ITO conductive glass is then transferred to a glove box filled with an inert gas, PVK dissolved in a chlorobenzene solution is spin-coated on the PEDOT:PSS film, followed by annealing to form a PEDOT:PSS / PVK layer, which is used as a hole injection layer and a hole transport layer; Spin-coat the exciplex mixed solution prepared in step 2 onto the PEDOT:PSS / PVK layer as a light-emitting layer; Step 4: Transfer the product obtained in step 3 into a vacuum chamber, and sequentially deposit TPBi, LiF and Al layers by thermal evaporation, wherein the TPBi layer serves as an electron transport layer and a hole blocking layer, and the LiF and Al layers serve as top electrodes; thus, a light-emitting device based on an exciplex is obtained.
2. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: In step 2, the addition ratio of PO-T2T solution and BCzPh solution is 1:
1.
3. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: In step 2, the stirring time is 5 min under an inert gas environment at room temperature, and the stirring speed is 600-1000 r / min.
4. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: In step 1, the concentration ratio of BCzPh to PO-T2T is 1:1, and the volume ratio is 1:
1.
5. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: The inert gas in steps 1-3 is nitrogen.
6. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: In step 3, the rotation speed of spin coating PeDOT:PSS is 2000 r / min, the rotation speed of spin coating PVK is 2000 r / min, and the rotation speed of spin coating the exciplex solution on the PeDOT:PSS / PVK layer is 1500 r / min.
7. The method for preparing a light-emitting device based on an exciplex according to claim 1, characterized in that: In step 3, the annealing treatment of PeDOT:PSS is specifically: annealing at a temperature of 170°C for 30 minutes; the annealing treatment of PVK is specifically: annealing at a temperature of 150°C for 15 minutes.
Citation Information
Patent Citations
Preparation method of full-solution method exciplex OLED
CN109378406A
Dark blue photo-thermal cross-linking type thermal activation delayed fluorescence material, and preparation method and application thereof
CN111606841A
Quaternary exciplex-based organic white light electroluminescent device with single light-emitting layer and preparation method of quaternary exciplex-based organic white light electroluminescent device
CN116133453A
Organic light emitting diode (OLED) device without blue light harm and application thereof
CN117440701A
Organic light-emitting composite material and an organic light-emitting device comprising the same
US20200321539A1