Injection molded article and method for producing injection molded article

By using thermoplastic resin, thermoplastic starch and carbodiimide compound in bioplastic injection molding products, combining the design of thick and thin walls, the color change is achieved using temperature differences, and the problem of high cost of bioplastic injection molding products is solved. , creates highly designed and environmentally friendly products.

CN119053425APending Publication Date: 2024-11-29HITACHI LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380035574.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-22
Filing Date
2023-03-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The high cost of bioplastic injection molded products limits their application in design and environmental value, and the prior art is difficult to manufacture products with high design at low cost.

Method used

Use thermoplastic resin, thermoplastic starch and compounds with carbodiimide groups as components, and create thick and thin wall parts in injection molded products, and use the temperature difference generated by shear heating to achieve a high design ability. Products do not require subsequent coating processes.

Benefits of technology

It has achieved the manufacture of high-designable bioplastic injection molded products at low cost, with biodegradability and carbon neutrality effects, and enhanced tone changes through temperature differences, significantly improving the design value of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053425A_ABST
    Figure CN119053425A_ABST
Patent Text Reader

Abstract

An injection-molded article containing a thermoplastic resin, a thermoplastic starch, and a compound having a carbodiimide group, the injection-molded article having a thick portion and a thin portion, the brightness of the thick portion being greater than the brightness of the thin portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an injection molded product and a method for producing the injection molded product. Background Art

[0002] Injection molded products made of plastic (resin materials) are used in a wide range of applications. In recent years, injection molded products using bioplastics (a general term for plastics made from biomass and biodegradable plastics) have been developed to reduce the impact of plastic waste on the environment.

[0003] For example, Patent Document 1 describes a method for producing an injection molding material, which includes a mixing step of mixing fibrillated cellulose, a hydrophobic biodegradable material, and starch in air.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-60697 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Bioplastics are generally expensive, and therefore it is desired to impart added value other than environmental value such as high design properties to bioplastic injection-molded products and to manufacture them at low cost.

[0009] An object of the present invention is to produce a bioplastic injection-molded product with high design at low cost.

[0010] Methods for solving problems

[0011] An injection molded article according to one embodiment of the present invention includes a thermoplastic resin, thermoplastic starch, and a compound having a carbodiimide group, and has a thick portion and a thin portion, wherein the brightness of the thick portion is greater than that of the thin portion.

[0012] Effects of the Invention

[0013] According to one embodiment of the present invention, a bioplastic injection-molded product with high design properties can be manufactured at low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic cross-sectional view of an example of an injection molding device used for producing an injection molded product according to an embodiment.

[0015] Figure 2 This is a schematic diagram showing the appearance of the injection-molded product of Example 1.

[0016] Figure 3This is a photograph of an injection-molded product made from the material of Comparative Example 1.

[0017] Figure 4 This is a photograph of an injection-molded product made from the material of Comparative Example 2.

[0018] Figure 5 This is a photograph of an injection molded product made from the material of Example 1.

[0019] Figure 6 This is a photograph of an injection molded product made from the material of Example 2.

[0020] Figure 7 This is a graph showing the relative color difference of injection molded products produced from the materials of Examples 1 and 2 and Comparative Examples 1 and 2.

[0021] Figure 8 This is a graph showing the tensile strength of injection molded products produced from the materials of Examples 1 and 2 and Comparative Examples 1 and 2.

[0022] Fig. 9A This is a schematic diagram showing the appearance of the injection-molded product of Example 3.

[0023] Fig. 9B This is a schematic diagram showing the appearance of the injection-molded product of Example 3.

[0024] Fig.10 It is a figure which shows the structure of the mold used for injection molding. DETAILED DESCRIPTION

[0025] Hereinafter, the embodiments will be described with reference to the accompanying drawings as appropriate. In the drawings referred to in the following description, the same components or components having the same functions are marked with the same figure numerals, and repeated descriptions are sometimes omitted. In addition, for the convenience of explanation, the dimensional ratio of the drawings is sometimes different from the actual ratio, or a part of the components is omitted from the drawings. In this application, the numerical range represented by the symbol "~" includes the numerical values ​​recorded before and after the symbol "~" as the lower limit and upper limit, respectively. In addition, the present invention is not limited to the following embodiments, and various design changes can be made without departing from the spirit of the present invention described in the claims.

[0026] First embodiment

[0027] The injection molded product of the first embodiment includes a thermoplastic resin as a first component, a thermoplastic starch (hereinafter, referred to as TPS) as a second component, and a compound having a carbodiimide group (hereinafter, referred to as a carbodiimide compound) as a third component. In addition, there are one or more thick-walled portions and thin-walled portions in the injection molded product.

[0028] Reference Figure 2, the structure of the injection molded product of the first embodiment is described.

[0029] The injection molded product of the first embodiment is an injection molded product containing a thermoplastic resin, thermoplastic starch, and a compound having a carbodiimide group.

[0030] like Figure 2 As shown, the injection molded product has a thick portion 201 and a thin portion 202. The brightness of the thick portion 201 is greater than that of the thin portion 202. Specifically, the difference between the relative color difference of the thick portion 201 and the relative color difference of the thin portion 202 is ΔE=1.0 or more.

[0031] In the injection molding described later, an injection molded product having a desired three-dimensional shape is produced by flowing resin into a mold of a predetermined shape and cooling and solidifying it. At this time, in the thin-walled part, the so-called shear heating caused by the friction heat between the flowing resin and the mold wall surface is significantly generated compared to the thick-walled part, so the resin of the thin-walled part 202 is molded at a higher temperature than the resin of the thick-walled part 201. However, the maximum temperature difference that can be achieved by shear heating is about 30°C, and even if the general resin material is molded using this temperature difference, a significant color difference cannot be obtained. Therefore, in the present invention, by using TPS and carbodiimide compounds as components, the degree of color change is enhanced by using temperature difference, and an injection molded product with a significant color difference due to wall thickness is realized. As a result, patterns, designs, and images can be formed without subsequent processes such as painting, and injection molded products with high design properties can be obtained at a low cost.

[0032] TPS may contain starch and a plasticizer. TPS may be obtained by mixing starch and a plasticizer.

[0033] Starch can come from plants, for example, it can come from cereals such as corn, wheat, and rice, beans such as broad beans, mung beans, and red beans, tubers such as potatoes, sweet potatoes, and cassava, wild grasses such as pigweed, bracken, and kudzu, and coconuts such as sago palm.

[0034] The plasticizer may be a compound having a functional group (e.g., hydroxyl, amino, carboxyl) that can form a hydrogen bond with the functional group of starch. Examples of plasticizers include glycols such as glycerol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, butylene glycol, polyglycerol, and thiodiglycol.

[0035] Sugars such as glucose, fructose, sucrose, galactose, maltose, lactose, trehalose, etc., sugar alcohols such as sorbitol, maltitol, xylitol, erythritol, mannitol, lactitol, sugar derivatives such as sucralose, hydroxy acids such as tartaric acid, polyols such as polyvinyl alcohol, trehalose, polyhydroxy (meth) acrylate, polyamines such as urea and thiourea, polycarboxylic acids such as hyaluronic acid, polyvinyl pyrrolidone, and mixtures thereof.

[0036] TPS is derived from biomass, is biodegradable, and is inexpensive. Therefore, the injection molded article of this embodiment can contribute to carbon neutrality, at least a portion of which can be biodegradable, and can be manufactured at low cost.

[0037] When the granular starch that has not been thermoplasticized is used in a compound or in an injection molding device as described later, it is possible that the screw may be clogged, but there is no such concern for the TPS processed by the pellets. Therefore, the injection molded product of the present embodiment including the TPS can be manufactured by an injection molding device as described later.

[0038] The thermoplastic resin of the first component can be, for example, polypropylene (PP), polyethylene (PE), polystyrene (PS), acrylonitrile-butadiene-styrene copolymer (ABS), polymethyl methacrylate (PMMA), polylactic acid (PLA), polybutylene succinate (PBS), hydroxybutyrate hydroxyhexanoate (PHBH), polyhydroxyalkanoic acid (PHA), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and polyvinyl alcohol (PVA).

[0039] The thermoplastic resin of the first component may be biodegradable. Thus, all or part of the injection molded product may be biodegradable. Examples of biodegradable resins include PLA, PBS, PHBH, PHA, PVA, PBSA, and PBAT. The thermoplastic resin of the first component or polyesters such as PLA, PBS, PHBH, PHA, PBSA, and PBAT may also be used. The thermoplastic resin of the first component or a biodegradable polyester may also be used.

[0040] The thermoplastic resin of the first component may be a mixture of a thermoplastic resin that is not biodegradable and a biodegradation accelerator. The biodegradation accelerator may be, for example, a microorganism involved in biodegradation, an enzyme, a substance that induces microorganisms, or a substance that promotes resin hydrolysis. Thus, all or part of the resin molding may be biodegradable.

[0041] The thermoplastic resin of the first component may be derived from biomass. This can improve carbon neutrality. Examples of biomass-derived resins include biomass-derived PLA, PBS, PHBH, PHA, PE, PP, and PS.

[0042] Examples of the carbodiimide compound include (“CARBODILITE” manufactured by Nisshinbo Chemical Co., Ltd., etc.).

[0043] The injection molded product of this embodiment may further include an additive. The additive is preferably a material that does not promote yellowing of TPS and does not react with TPS to form a gel. In addition, the additive is preferably a material that is not derived from petroleum, such as an inorganic substance.

[0044] As another example of an additive, an antibacterial agent can be cited. A resin molding containing an antibacterial agent can prevent or reduce contamination by microorganisms in the use environment, and can therefore be applied to food-related uses (e.g., food containers). As examples of antibacterial agents suitable for food-related uses, antibacterial agents having silver-based inorganic compounds or zinc oxide-based compounds as main components can be cited. The content of the antibacterial agent can be appropriately set according to the mechanical properties of the resin molding, for example, it can be 0.1 to 1.0 parts by weight relative to 100 parts by weight of the total weight of the first thermoplastic resin, the second thermoplastic resin, and TPS.

[0045] Other examples of the additive include fillers, heat stabilizers, lubricants, mold release agents, nucleating agents, photodegradants, biodegradation accelerators, antioxidants, ultraviolet stabilizers, antistatic agents, flame retardants, and deodorants.

[0046] In the injection molded article of this embodiment, the color tone of the thick portion 201 and the color tone of the thin portion 202 preferably have a relative color difference of ΔE=1.0 or more in the CIELAB color space. By achieving such a relative color difference, the color tones of the thick portion 201 and the thin portion 202 can be clearly distinguished by naked eyes.

[0047] The method for manufacturing an injection molded product of the present embodiment is described below. The method for manufacturing an injection molded product includes performing injection molding using pellets containing TPS and a carbodiimide compound. As an example of the manufacturing method, the following describes a method using Figure 1 A method for manufacturing an injection molded product using the injection molding apparatus shown.

[0048] First, raw material pellets 104 are supplied to the hopper 103 of the injection molding device 100. The raw material pellets 104 contain pellets containing TPS. The pellets containing TPS may be pellets containing TPS as the main component, or may be composite pellets containing at least one of the thermoplastic resin or carbodiimide compound of the first component and TPS. The pellets containing TPS as the main component may be produced by supplying starch and a plasticizer to an extrusion molding device and mixing, extruding, and cutting. Commercially available TPS pellets may also be used. Composite pellets containing at least one of the thermoplastic resin or carbodiimide compound of the first component and TPS may be produced by supplying at least one of the thermoplastic resin or carbodiimide compound of the first component and TPS pellets to an extrusion molding device and mixing, extruding, and cutting.

[0049] The raw material pellets 104 may contain at least one of pellets of a thermoplastic resin of the first component, pellets of a carbodiimide compound, or composite pellets of a thermoplastic resin of the first component and a carbodiimide compound in addition to the pellets containing TPS. Furthermore, an additional material may be supplied to the hopper 103 as needed.

[0050] The screw 102 is retracted by the motor 101, and the raw material pellets 104 are introduced from the hopper 103 to the cylinder 106. The raw material pellets 104 are heated by the heater 105 while the screw 102 is rotated, so that the raw material pellets 104 are melted. The temperature (molding temperature) of the heater 105 is preferably below 230°C, and more preferably below 210°C. In this way, thermal degradation and yellowing of TPS can be prevented or reduced. In addition, as needed, supercritical fluids such as nitrogen and carbon dioxide can be further introduced into the cylinder 106 and mixed with the melt of the raw material pellets 104. In this way, it is easy to manufacture resin molded products with a small thickness and injection molded products with complex shapes.

[0051] Next, the screw 102 is advanced by the motor 107, and the melt in the cylinder 106 is ejected into the mold 109 through the nozzle 108. After the mold 109 is filled with the melt, a predetermined pressure is applied to further supply the melt to the mold 109 in order to compensate for the volume shrinkage caused by the subsequent solidification of the melt.

[0052] By maintaining the mold 109 at a predetermined temperature, the melt is cooled to a solidification temperature or lower and solidified.

[0053] The mold clamping mechanism 111 is driven by the motor 110 to open the mold 109. Then, the ejection mechanism 113 is driven by the motor 112 to remove the solidified product (resin molded product) from the mold 109. Finally, the mold 109 is closed to prepare for the next injection molding. In this way, the injection molded product of the first embodiment is manufactured.

[0054] Second embodiment

[0055] In the injection molded product of the second embodiment, the thermoplastic resin of the first component is a mixture of two or more thermoplastic resins. Here, the two mixed thermoplastic resins may be dissolved to form a single phase, or separated and dispersed into multiple phases. The examples of the two or more thermoplastic resins are the same as the examples of the thermoplastic resin of the first component described above.

[0056] In the injection molded article of the second embodiment, the difference in solubility parameters (SP values) between the two or more thermoplastic resins constituting the thermoplastic resin of the first component may be 1.0 (J / cm 3 ) 0.5 the following.

[0057] It should be noted that the SP value in the present invention can be obtained by a method of estimating from the molecular structure of the compound or a method of estimating from the physical property values ​​of the compound. Examples of methods of estimating from the molecular structure of the compound include Small's calculation method, Rheineck and Lin's calculation method, Krevelen and Hoftyzer's calculation method, Fedors' calculation method (RF Fedors, Polym. Eng. Sci., 14 (2), 147 (1974)), Hansen's calculation method (CM Hansen, J. Paint Technol., 39., (505), 104 (1967)) and Hoy's calculation method (HL Hoy, J. Paint Technol., 42 (540), 76 (1970)). Examples of methods for estimating from the physical property values ​​of a compound include a method of determining from latent heat of vaporization, a method based on the Hildebrand Rule (J. Hildebrand and R. Scott, "The Solubility of Non-electrolytes", 3rd Ed., pp. 119-133, Reinhold Publishing Corp. (1949)), a method based on surface tension, a method of determining from a solubility value, a method of determining from a refractive index, and a method of determining from other physical property values.

[0058] Third embodiment

[0059] like Fig. 9A , Fig. 9B As shown, the injection molded product of the third embodiment can be arranged so that the thin-walled portion 202 and the thick-walled portion 201 have periodicity. With such a configuration, portions with different hues appear periodically, and a highly designed pattern can be expressed on the surface of the injection molded product.

[0060] In the injection molded article of the second embodiment, the thin-walled portion 202 and the thick-walled portion 201 may be arranged to form a periodic stripe pattern (see Fig. 9A ) or a checkered pattern (see Fig. 9B ).

[0061] Fourth embodiment

[0062] In the fourth embodiment, referring to Fig.10 The structure of the mold used for injection molding will be described.

[0063] In injection molding, a resin in a fluid state is poured into a mold 1010 of a predetermined shape, and is cooled and solidified, thereby manufacturing an injection molded product having a desired three-dimensional shape.

[0064] The unique pattern of bioplastics (which are prone to change color due to heat) is formed by shear heat. In particular, when carbodiimide compounds are added, the color change caused by temperature is easily enhanced.

[0065] like Fig.10 As shown, in the thin part of the mold, the friction heat (shear heating) generated between the flowing resin and the wall surface becomes larger, and the resin temperature rises by about 5-20° C. The color of starch changes sensitively with temperature, so a pattern corresponding to the shape of the mold 1010 can be formed.

[0066] Thus, in the fourth embodiment, a mold 1010 of a predetermined shape is used to manufacture an injection molded product. Fig.10 As shown, a mold having a thin portion and a thick portion is used as the mold 1010. The high temperature portion 1020 is formed by the thin portion of the mold 1010 during injection molding. In addition, the low temperature portion 1030 is formed by the thick portion of the mold 1010 during injection molding.

[0067] In this way, a pattern corresponding to the shape of the mold 1010 is formed on the injection molded product. The pattern corresponding to the shape of the mold 1010 is, for example, a periodic stripe pattern (see Fig. 9A ) or a checkered pattern (see Fig. 9B ).

[0068] Then, the mold 1010 is used to perform injection molding in a state where the high temperature portion 1020 and the low temperature portion 1030 are formed on the injection molded product. At this time, the brightness of the low temperature portion 1030 during injection molding of the injection molded product is greater than the brightness of the high temperature portion 1020 .

[0069] High temperature portion 1020 during injection molding of injection molded product (refer to Fig.10 ) After injection molding, a thin-walled portion 202 is formed (refer to Figure 2 ). Low temperature portion 1030 during injection molding of injection molded product (refer to Fig.10 ) After injection molding, a thick wall portion 201 is formed (refer to Figure 2 ).

[0070] Example

[0071] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples.

[0072] (1) Production of injection molded products

[0073] (Comparative Example 1)

[0074] The PP pellets and TPS pellets in the amounts listed in Table 1 were supplied to an extruder, and extrusion molding was performed at a temperature of 160 to 180°C to obtain composite pellets. The composite pellets were supplied to an injection molding machine, and injection molding was performed to obtain injection molded products. It should be noted that, in order to confirm the degree of color tone change caused by temperature change, instead of making injection molded products with thick wall parts 201 and thin wall parts 202, multiple test pieces with constant wall thickness and changed molding temperatures were made. The temperature of the multiple heaters of the injection molding machine was 170 to 210°C, and the temperature was higher the closer to the injection nozzle.

[0075] (Comparative Example 2)

[0076] The amount of PLA particles, PBS particles, and TPS particles recorded in Table 1 are supplied to an extruder, and extrusion molding is performed at a temperature of 160 to 180°C to obtain composite particles. The composite particles are supplied to an injection molding machine, and injection molding is performed to obtain injection molded products. It should be noted that in order to confirm the degree of color tone change caused by temperature changes, instead of making injection molded products with thick wall parts 201 and thin wall parts 202, multiple test pieces with constant wall thickness and changed molding temperatures were made. The temperature of the multiple heaters of the injection molding machine is 170 to 210°C, and the temperature is higher the closer to the injection nozzle.

[0077] (Example 1)

[0078] The amounts of PP particles, TPS particles and carbodiimide compounds ("CARBODILITE" manufactured by Nisshinbo Chemical Co., Ltd.) listed in Table 1 were supplied to an extruder, and extrusion molding was performed at a temperature of 160 to 180°C to obtain composite particles. The composite particles were supplied to an injection molding machine, and injection molding was performed to obtain injection molded products. It should be noted that, in order to confirm the degree of color tone change caused by temperature changes, instead of making injection molded products with thick-walled portions 201 and thin-walled portions 202, multiple test pieces with constant wall thickness and changed molding temperatures were made. The temperature of the multiple heaters of the injection molding machine was 170 to 210°C, and the temperature was higher the closer to the injection nozzle.

[0079] (Example 2)

[0080] The amounts of PLA particles, PBS particles, TPS particles and carbodiimide compounds (CARBODILITE manufactured by Nisshinbo Chemical Co., Ltd.) listed in Table 1 are supplied to an extruder, and extrusion molding is performed at a temperature of 160 to 180°C to obtain composite particles. The composite particles are supplied to an injection molding machine, and injection molding is performed to obtain injection molded products. It should be noted that, in order to confirm the degree of color tone change caused by temperature changes, instead of making injection molded products with thick-walled portions 201 and thin-walled portions 202, multiple test pieces with constant wall thickness and changed molding temperatures were made. The temperature of the multiple heaters of the injection molding machine is 170 to 210°C, and the temperature is higher the closer to the injection nozzle.

[0081] [Table 1]

[0082]

[0083] *Amount relative to the total weight of PP, PLA, PBS and TPS

[0084] **Amount relative to 100 parts by weight of the total weight of PLA, PBS and TPS

[0085] (2) Appearance observation and color tone measurement

[0086] A schematic diagram showing the appearance of the injection molded product of Example 1 is shown in Figure 2 The materials of Comparative Example 1, Comparative Example 2, Example 1, and Example 2 were used to produce injection molded products using molding temperature as a parameter. Figure 3 , Figure 4 , Figure 5 , Figure 6 .like Figure 2 As shown, in the injection molded product of Example 1, the brightness of the thick wall portion 201 is higher than that of the thin wall portion 202, and the appearance of the pattern based on the color tone difference can be recognized. Figure 3 , Figure 4 As shown in FIG. 1 , in the injection molded products made with the material compositions of Comparative Examples 1 and 2, even when the molding temperature is changed from 170°C to 210°C, there is almost no difference in color tone. Figure 5 , Figure 6 As shown in FIG. 1 , the injection molded products made from the material compositions of Examples 1 and 2 have enhanced the color tone change based on the molding temperature compared to Comparative Examples 1 and 2. The relative color tones of the injection molded products made from the materials of Examples 1 and 2 and Comparative Examples 1 and 2 were measured in the CIELAB color space, and the results are shown in FIG. Figure 7The relative color difference of Comparative Examples 1 and 2 changed by less than ΔE=1.0 per 20°C temperature difference, but the relative color difference of Examples 1 and 2 changed by more than ΔE=4.0 per 20°C temperature difference, and the relative color difference based on temperature change was enhanced.

[0087] (3) Mechanical properties evaluation

[0088] The tensile strength of the injection molded products made from the materials of Examples 1 and 2 and Comparative Examples 1 and 2 was measured in accordance with ISO527. The results are shown in Figure 8 .

[0089] The injection molded article produced from the material of Example 1 has a tensile strength equivalent to that of Comparative Example 1. The injection molded article produced from the material of Example 2 has a tensile strength equivalent to that of Comparative Example 2.

[0090] (4) Examples of periodic patterns

[0091] A schematic diagram showing the appearance of the injection molded product of Example 3 is shown in Fig. 9A , Fig. 9B As an injection molded product having a periodic pattern, for example, Fig. 9A The striped pattern shown or Fig. 9B Injection molded product with the lattice pattern shown.

[0092] According to the above-described embodiment, a bioplastic injection-molded product with high design properties can be manufactured at low cost.

[0093] Description of Reference Numerals

[0094] 100: injection molding device, 101, 107, 110, 112: motor, 102: screw, 103: hopper, 104: raw material particles, 105: heater, 106: cylinder, 108: nozzle, 109: mold, 111: mold clamping mechanism, 113: ejection mechanism.

Claims

1. An injection molded product, characterized in that It contains thermoplastic resin, thermoplastic starch and a compound having a carbodiimide group. The injection molded product has a thick wall portion and a thin wall portion, and the brightness of the thick wall portion is greater than the brightness of the thin wall portion.

2. The injection molded article according to claim 1, characterized in that The difference between the relative color difference of the thick portion and the relative color difference of the thin portion is ΔE=1.0 or more.

3. The injection molded article according to claim 1, wherein: The thermoplastic resin is a polyester resin.

4. The injection molded article according to claim 1, wherein: The thermoplastic resin is a polyolefin resin.

5. The injection molded article according to claim 1, wherein: The thermoplastic resin is a mixture of multiple thermoplastic resins.

6. The injection molded article according to claim 1, wherein: The thick-walled portion and the thin-walled portion are arranged with a predetermined periodicity.

7. A method for manufacturing an injection molded product, characterized in that: The present invention relates to a method for producing the injection molded article according to claim 1, wherein the injection molding is performed using pellets containing the thermoplastic resin, the thermoplastic starch and the compound having a carbodiimide group.

8. The method for manufacturing an injection molded product according to claim 7, wherein: The injection molding is performed in a state where a high temperature portion and a low temperature portion are formed on the injection molded product, and brightness of the low temperature portion during injection molding of the injection molded product is greater than brightness of the high temperature portion.

9. The method for manufacturing an injection molded product according to claim 8, wherein: The high temperature portion of the injection molded product during the injection molding forms the thin wall portion after the injection molding, and the low temperature portion of the injection molded product during the injection molding forms the thick wall portion after the injection molding.

10. The method for manufacturing an injection molded product according to claim 9, wherein: The injection molded product is manufactured using a mold of a predetermined shape.

11. The method for manufacturing an injection molded product according to claim 10, wherein: As the mold, a mold having a thin portion and a thick portion is used, the high temperature portion is formed by the thin portion of the mold during the injection molding, and the low temperature portion is formed by the thick portion of the mold during the injection molding.

12. The method for manufacturing an injection molded product according to claim 10, wherein: A pattern corresponding to the shape of the mold is formed on the injection molded product.

13. The method for manufacturing an injection molded product according to claim 12, wherein: The pattern corresponding to the shape of the mold is a stripe pattern or a lattice pattern having a periodicity.

Citation Information

Patent Citations