Lateral gap filling
Through ALD technology and suppression operation, gap filling is achieved in semiconductor equipment without gaps, solving the problems of gaps and joints in film gaps, and improving the uniformity and quality of the film.
Patent Information
- Application Number
- CN202380035405.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-29
AI Technical Summary
In semiconductor devices, high-quality films often face problems in forming voids and joints, especially in the process of filling the film with uniformity and gapless deposition.
Atomic layer deposition (ALD) technology combined with suppression operation ensures bottom-to-top or Fill from the inside to the outside.
The gap filling without voids is achieved, the formation of seams is reduced, the uniformity and quality of the film is improved, and the control of deposition is enhanced.
Smart Images

Figure CN119054047A_ABST
Abstract
Description
Related Applications
[0001] The PCT application form is filed concurrently with this specification as a part of this application. Each application identified in the concurrently filed PCT application form to which this application claims the benefit or priority is incorporated herein by reference in its entirety. Background Art
[0002] Many semiconductor device processes involve film formation, including silicon-containing films such as silicon oxide or silicon nitride. Depositing high-quality films can be particularly challenging when depositing films in gaps. Challenges can include the formation of voids and / or seams in the film.
[0003] The background description provided here is for the purpose of generally presenting the context of the present disclosure. The work of the presently designated inventors is neither explicitly nor implicitly admitted to be prior art against the present disclosure to the extent that it is described in this background section and to aspects of the specification that could not be determined as prior art at the time of filing the application. Summary of the invention
[0004] Aspects of the present disclosure relate to atomic layer deposition (ALD) of dielectric material within a gap that facilitates void-free bottom-up or inside-out gap filling. One or more inhibition operations are performed during the gap filling. The inhibition operations modify the surface of the gap in a manner that inhibits growth in subsequent ALD cycles.
[0005] One aspect of the present disclosure relates to a method of filling a feature of a structure on a substrate in a chamber, the method comprising: performing one or more cycles of the following steps: (a) providing a halogen-containing gas to the chamber in the absence of a plasma to inhibit deposition on at least a portion of the feature; (b) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
[0006] In some embodiments, the dielectric material is an oxide, a nitride, or a carbide. In some embodiments, the method further comprises, prior to performing one or more cycles of (a) and (b), depositing a liner layer in the feature by atomic layer deposition.
[0007] In some embodiments, operation (a) results in self-limiting etching.
[0008] In some embodiments, operation (a) produces a halogen-terminated surface.
[0009] In some embodiments, the method further comprises providing water, or one or more reactants capable of forming water, to the chamber. In some embodiments, operation (b) comprises providing a halogen-containing gas, hydrogen (H2) and oxygen (O2) to the chamber.
[0010] In some embodiments, the structure includes a vertically oriented feature having a plurality of sidewalls, a plurality of openings in the sidewalls creating a plurality of laterally oriented features fluidically accessible through the plurality of openings, wherein the feature is one of the laterally oriented features.
[0011] In some embodiments, the method further comprises performing one or more cycles of: (c) providing a halogen-containing gas or a halogen-free gas to the chamber under plasma conditions to inhibit deposition on at least a portion of the feature; (d) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
[0012] According to various embodiments, the cycles of (c) and (d) may be performed before, after, or interleaved with the cycles of (a) and (d).
[0013] Another aspect of the present disclosure relates to an apparatus comprising: a chamber for containing a substrate; a gas inlet for admitting a gas into the chamber; and a controller comprising a plurality of instructions for: (a) providing a halogen-containing gas to the chamber in the absence of a plasma to inhibit deposition on at least a portion of the feature; (b) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
[0014] Another aspect of the present disclosure relates to a method of filling a feature of a structure on a substrate in a chamber, comprising performing one or more inhibit-deposition cycles of: (a) providing a plasma to the chamber, the plasma generated from a nitrogen-containing and halogen-free gas, thereby inhibiting deposition on at least a portion of the feature, wherein during (a), the pressure of the chamber is at least 5 Torr; and (b) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
[0015] In some embodiments, the dielectric material is an oxide, a nitride, or a carbide. In some embodiments, the method further comprises, prior to performing one or more inhibit-deposition cycles of (a) and (b), depositing a liner layer in the feature by atomic layer deposition.
[0016] In some embodiments, the structure includes a vertically oriented feature having an opening that creates a plurality of laterally oriented features accessible to a fluid through the plurality of openings, wherein the feature is one of the laterally oriented features. In some embodiments, the vertically oriented feature has a depth of at least 1 micron. In some embodiments, the vertically oriented feature has a depth of at least 2 microns.
[0017] In some embodiments, (b) comprises one or more plasma enhanced atomic layer deposition cycles. In some such embodiments, the plasma power during (b) is higher than the plasma power during (a). In some embodiments, (b) comprises one or more thermal atomic layer deposition cycles.
[0018] In some embodiments, (b) is performed only once per inhibition-deposition cycle. In some embodiments, the duration of (a) is at least 10 seconds per inhibition-deposition cycle. In some embodiments, the duration of (a) is at least 20 seconds per inhibition-deposition cycle. In some embodiments, the duration of (a) is at least 30 seconds per inhibition-deposition cycle. In some embodiments, the plasma in (a) is generated from N2 gas. In some embodiments, the plasma in (a) is generated from a mixture of N2 gas and hydrogen (H2). In some embodiments, the plasma in (a) is generated from NH3 gas. In some embodiments, the plasma in (a) densifies the dielectric film in the laterally oriented features.
[0019] Another aspect of the present disclosure relates to a method comprising providing a substrate having a structure to a processing chamber, the structure comprising a vertically-oriented feature, a plurality of openings in the vertically-oriented feature creating a plurality of laterally-oriented features accessible to a fluid through the plurality of openings, wherein the vertically-oriented feature has a depth of at least one micron; and performing a plurality of cycles of: (a) exposing the substrate to a plasma generated from N2 to selectively suppress a portion of the laterally oriented features, wherein during (a), the pressure of the processing chamber is at least about 5 Torr, and wherein the duration of (a) is at least about 10 seconds; and (b) After (a), a plasma enhanced atomic layer deposition process is performed to deposit a dielectric material in the laterally oriented features, wherein the plasma power in (a) is less than the plasma power in (b).
[0020] In some embodiments, the plasma in (a) densifies the dielectric film in the laterally oriented features.
[0021] Another aspect of the present disclosure relates to a method comprising providing a substrate having a structure to a processing chamber, the structure comprising a vertically-oriented feature, a plurality of openings in the vertically-oriented feature creating a plurality of laterally-oriented features accessible to a fluid through the plurality of openings, wherein the vertically-oriented feature has a depth of at least one micron; and performing a plurality of cycles of: (a) exposing the substrate to a suppression plasma to selectively suppress a portion of the laterally oriented features; and (b) Following (a), an atomic layer deposition process is performed to deposit dielectric material in the laterally directed features.
[0022] In some embodiments, the suppression plasma is halogen-free. In some embodiments, the suppression plasma is halogen-containing. In some embodiments, the suppression plasma is generated in a capacitively coupled plasma generator. In some embodiments, the suppression plasma is generated in an inductively coupled plasma generator. In some embodiments, the suppression plasma has a high radical density. In some embodiments, during (a), the pressure of the processing chamber is at least about 1 Torr.
[0023] Another aspect of the present disclosure relates to an apparatus comprising: a chamber for receiving a substrate; a plasma generator for generating plasma in the chamber; a gas inlet for admitting a gas into the chamber; and a controller comprising a plurality of instructions for: (a) providing a plasma to the chamber, the plasma generated from a nitrogen-containing and halogen-free gas, thereby inhibiting deposition on at least a portion of the feature, wherein during (a), the pressure of the chamber is at least 5 Torr; and (b) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
[0024] These and other features of the disclosed embodiments will be described in detail below with reference to the associated drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a diagram showing an example of a structure that may be filled with a dielectric material according to various embodiments.
[0026] Figure 2 is a diagram showing an example of a structure that may be filled with a dielectric material according to various embodiments.
[0027] Figure 3A is a flow chart showing an example method of filling a feature according to various embodiments.
[0028] Figure 3Bis an example showing a process sequence that may be used in accordance with the disclosed embodiments.
[0029] Figure 4 is a graph showing the thickness of the dielectric film as a function of the duration of the thermal inhibition treatment.
[0030] Figure 5 is a graph showing thickness after thermal inhibition and deposition.
[0031] Figure 6 is a flow chart showing an example method of filling a feature according to various embodiments.
[0032] Figure 7 is an example showing a process sequence that may be used in accordance with the disclosed embodiments.
[0033] Figure 8 is a flow chart showing an example method of atomic layer deposition (ALD) according to various embodiments.
[0034] Fig. 9 is a schematic diagram of an example processing station for performing the disclosed embodiments.
[0035] Figures 10 to 12 is a schematic diagram of an exemplary processing tool for performing the disclosed embodiments. DETAILED DESCRIPTION
[0036] In the following description, numerous specific details are set forth to provide a thorough understanding of the embodiments presented. The disclosed embodiments may be implemented without some or all of these specific details. In other cases, well-known processing operations are not described in detail to avoid unnecessarily obscuring the disclosed embodiments. Although the disclosed embodiments will be described in conjunction with specific embodiments, it should be understood that they are not intended to limit the disclosed embodiments.
[0037] Semiconductor manufacturing processes typically include dielectric gap filling of features using chemical vapor deposition (CVD) and / or atomic layer deposition (ALD) methods. Methods of filling features using dielectric materials (including but not limited to silicon-containing films, such as silicon oxides), and related systems and devices are disclosed herein. The methods described herein can be used to fill features formed in a substrate. Such features may be referred to as gaps, recessed features, negative features, unfilled features, or simply features. Filling such features may be referred to as gap filling. Features formed in a substrate may be characterized by one or more narrow and / or concave openings, constrictions within the feature, and a high aspect ratio. In certain embodiments, the feature may have an aspect ratio of at least about 2:1, at least about 4:1, at least about 6:1, at least about 20:1, at least about 100:1, or greater. The substrate may be a silicon wafer such as a 200-mm wafer, a 300-mm wafer, a 450-mm wafer, which includes a wafer having one or more layers of material (e.g., dielectric, conductive or semiconductive material) deposited thereon.
[0038] One aspect of the present disclosure relates to atomic layer deposition (ALD) of a dielectric material in a gap, and the ALD promotes void-free bottom-up (or inside-out) gap filling. One or more inhibition operations are performed during the gap filling. The inhibition operation modifies the surface of the gap in a manner that inhibits growth in subsequent ALD cycles.
[0039] Examples of structures to be filled include 3D NAND structures, dynamic random access memory (DRAM) structures, and shallow trench isolation (STI) structures. These structures include multiple gaps, wherein the sidewalls of the gaps are formed of materials that are easily etched. In one embodiment, the 3D NAND structure includes an oxide-nitride-oxide-nitride (ONON) stack covered by a polysilicon layer. Other examples of sidewall materials include oxides, metals, and semiconductor materials.
[0040] According to various embodiments, these methods may be implemented to fill vertically oriented features and / or laterally oriented features. For example, in a vertical DRAM (VDRAM) structure, ALD may be used to fill laterally oriented trenches.
[0041] Although the embodiments herein are primarily described as filling features with dielectric materials in a void-free manner, in certain embodiments, these methods can be implemented to form air gaps in the features. In such embodiments, deposition can be suppressed over most or all of the features, thereby promoting pinch off at the top of the gap and the formation of voids or air gaps within the feature. In this way, capacitance can be reduced.
[0042] The features described herein generally have an opening and a plurality of sidewalls extending from the opening further into the feature. A vertically oriented feature has an axis extending from the opening and between the sidewalls, with the axis being oriented approximately orthogonal to the plane of the substrate. A laterally oriented feature has an axis extending from the opening and between the sidewalls, with the axis being oriented approximately parallel to the plane of the substrate.
[0043] Figure 1 An example of a portion of a VDRAM structure is shown, where the portion can be filled using the methods described herein. The structure includes multiple pairs, each pair including layer 104 and layer 106. Examples of materials for layer 104 include silicon germanium (SiGe), silicon nitride (SiN), and silicon dioxide (SiO2). Examples of materials for layer 106 include silicon (Si), silicon dioxide (SiO2), and silicon nitride (SiN). Laterally oriented features 114 are formed by etching and are to be filled with dielectric materials. Laterally oriented features 114 are formed in vertically oriented holes 108, which may also be referred to as vertically oriented features. Examples of the depth of vertically oriented features include at least 0.1 microns, at least 0.5 microns, at least 1 micron, at least 2 microns, at least 4 microns, and at least 5 microns. A VDRAM structure can have anywhere from a few pairs to hundreds of pairs. Exemplary depth-to-width ratios of vertically oriented trenches are at least 30:1, at least 50:1, at least 100:1, or higher. Example opening widths of the laterally oriented features are 5 to 20 nm. Example aspect ratios of the laterally oriented features are at least 10:1, at least 20:1, or at least 25:1.
[0044] The laterally oriented features 114 are fluidically accessible via openings in the vertically oriented holes 108. In other words, if the laterally oriented features were not enclosed, gas could enter the laterally oriented features. Void-free filling by ALD relies on having a sufficient amount of the deposition precursor migrate through the vertically oriented holes 108, the openings of the laterally oriented features 114, and into the furthest reaches of the laterally oriented features before cumulative deposition of dielectric material that could pinch off the openings and prevent further migration of the precursor into the laterally oriented features 114.
[0045] Filling with ALD Figure 1 The structure shown is challenging. While ALD can result in conformal growth on the structure, conformal growth from the sidewalls can create seams down the middle of the features. Additionally, achieving top-to-bottom uniformity so that laterally oriented features 114 near the bottom of the structure are filled to the same degree as laterally oriented features 114 near the top of the structure is difficult.
[0046] Lateral gap filling presents challenges that are not encountered when filling vertically oriented features. For example, a plasma suppression operation may be used during ALD to fill vertically oriented features. The suppressor plasma creates a passivated surface and increases the nucleation barrier for the deposited ALD film. When the suppressor plasma interacts with the material in the feature, the material at the bottom of the feature receives less plasma treatment than the material near the top of the feature or in the field region due to geometric shielding effects. As a result, deposition at the top of the feature is selectively suppressed, while deposition in the lower portion of the feature proceeds with less or no suppression. Filling from the bottom up is enhanced, resulting in a more favorable sloped profile that mitigates seam effects and prevents void formation.
[0047] However, if a similar process is used to fill Figure 1 In the VDRAM structure shown, the laterally oriented features at the bottom of the vertically oriented hole 108 may be more suppressed than those at the top. This will cause uneven filling between features. The methods described herein can be used for uniform top-down suppression and uniform filling between features.
[0048] Apart from Figure 1 In addition to the laterally oriented features in the examples of FIG. 1 , the gap filling process can also be used to fill other types of features that are challenging to fill. These features include high aspect ratio features, including vertically oriented features with aspect ratios of 10:1 or greater. In some embodiments, the feature to be filled is a concave feature. A concave feature is a feature that narrows at some point at the bottom or interior of the feature toward the opening. Figure 2 An example of a concave feature to be filled is shown. The feature includes a cusp 215 which may present a challenge to fill.
[0049] Described herein is a gap fill process that includes a thermal suppression operation or a plasma-based suppression operation. A thermal suppression operation is an operation that uses a non-plasma suppression gas. Plasma is not generated. A plasma-based suppression process uses a process gas, wherein the process gas includes plasma species, such as ions and / or radical species.
[0050] The thermal suppression process is described below with reference to FIGS. 3 to 5 , while the plasma suppression process is described below with reference to Figure 6 and 7 The atomic layer deposition process that can be used with the method of the present invention is described below. Figure 8 The device for implementing the method described herein is described in detail. Figures 9 to 12 And describe it.
[0051] Figure 3A is a process flow diagram that depicts a method for filling a gap with a dielectric material. The method begins with providing a structure having one or more gaps to be filled at operation 301. The structure can be formed from one or more material layers deposited on a substrate. The substrate can be a silicon or other semiconductor wafer, such as a 200 mm wafer, a 300 mm wafer, or a 450 mm wafer, including a wafer with one or more material layers (e.g., dielectric, conductive, or semiconductor materials) deposited thereon. These methods can also be applied to gap filling of other substrates, such as glass, plastic, etc., including for use in the manufacture of microelectromechanical (MEMS) devices.
[0052] Examples of structures include VDRAM structures, 3D NAND structures, and shallow trench isolation (STI) structures. The structure includes multiple gaps, wherein the sidewalls of the gaps are formed by materials that are easily etched. In some embodiments, the structure may include a lateral structure extending horizontally from a common vertical trench. Examples of sidewall materials include nitrides, oxides, metals, and semiconductor materials. The methods described herein are not limited to a specific type of sidewall material and can be used to inhibit any material that is easily etched.
[0053] In operation 305, a dielectric material is deposited in the gap using thermal suppression during fill. As discussed further below, this may involve cycles of atomic layer deposition (ALD) of the dielectric film followed by exposure to a suppression gas.
[0054] Thermal inhibition involves non-plasma exposure to a halogen-containing inhibition gas. The halogen-containing inhibition gas can be a fluorine (F)-containing gas, a chlorine (Cl)-containing gas, a bromine (Br)-containing gas, an iodine (I)-containing gas, or any combination thereof. Non-plasma conditions refer to conditions lacking plasma. In certain embodiments, one or more additional gases are introduced into the chamber so as to be present in the chamber with the halogen-containing gas. The one or more additional gases can flow into the chamber together with the halogen-containing gas or can be introduced separately.
[0055] The thermal inhibition operation can be performed on an existing formed dielectric material. In certain embodiments, the thermal inhibition results in the surface being at least partially terminated with a halogen.
[0056] In certain embodiments, the inhibitory species is generated within the reactor from a halogen-containing gas and one or more additional gases. For example, nitrogen trifluoride (NF3) and water (H2O) can react to generate hydrogen fluoride (HF), which can then react with the deposited film to form a fluorine-terminated film. In certain embodiments, hydrogen (H2) and oxygen (O2) are introduced into the chamber to form water. Other water sources may also be used.
[0057] In certain embodiments, HF or other inhibitory species that react with the deposited film is introduced by itself or only with an inert carrier or background gas.
[0058] In certain embodiments, the thermal inhibition operation may result in self-limiting etching of the existing formed dielectric material. For example, several angstroms of material may be etched, while the etched surface is fluorine terminated. This may inhibit subsequent deposition. Further discussion of halogen-containing gases and processing conditions during thermal inhibition is provided below.
[0059] Figure 3B An example of a processing sequence that can be used in accordance with certain embodiments is shown. Figure 3B In an exemplary processing sequence of FIG. 1 , a substrate such as a semiconductor wafer is provided for gap filling. The substrate may be provided to a deposition chamber after prior processing and / or maintained in a deposition chamber. At this stage, the substrate includes one or more features to be filled with a dielectric material. For example, a substrate having Figure 1 The substrate has a laterally oriented structure, or has Figure 2 A substrate with a gap having protruding portions is shown.
[0060] Next, n1 ALD deposition cycles are performed, where n1 is an integer of at least 1. ALD is a technique for sequentially depositing thin layers of material. The ALD process uses a surface-mediated deposition reaction to deposit films layer by layer in multiple cycles. The concept of an ALD "cycle" is relevant to the discussion of various embodiments herein. In general, a cycle is a minimum set of operations for performing a surface deposition reaction. The result of a cycle is the production of at least a portion of a silicon-containing film layer on the substrate surface. Typically, an ALD cycle includes the following operations: at least one reactant is delivered and adsorbed on the substrate surface, and then the adsorbed reactant is reacted with one or more reactants to form a partial film layer. The cycle may include certain auxiliary operations, such as sweeping one of the reactants or byproducts, and / or treating a portion of the film just deposited. Typically, a cycle includes an instance of a unique sequence of operations. For example, an ALD cycle may include the following operations: (i) delivery / adsorption of a precursor, (ii) removal of the precursor from the chamber, (iii) delivery of a second reactant (also referred to as a co-reactant), and (iv) removal of byproducts from the chamber. The reaction between the second reactant and the adsorbed precursor to form a film on the substrate surface can affect the composition and properties of the film, such as non-uniformity, stress, wet etch rate, dry etch rate, electrical properties (e.g., breakdown voltage and leakage current), etc. In a plasma enhanced ALD (PEALD) process, a plasma may be ignited during or after the delivery of the second reactant in (iii). A thermal ALD process is a non-plasma process. Figure 3BIn a related example, the ALD process is typically a thermal ALD process.
[0061] In one example of an ALD process, a substrate surface containing a population of surface active sites is exposed to a gas phase distribution of a first precursor (e.g., a silicon-containing precursor), wherein the first precursor is provided in a dose to a chamber containing the substrate. Molecules of the first precursor are adsorbed onto the substrate surface, including chemisorbed species and / or physisorbed molecules of the first precursor. When a compound is adsorbed onto the substrate surface as described herein, the adsorbed layer may include the compound, as well as derivatives of the compound. For example, an adsorbed layer of a silicon-containing precursor may include the silicon-containing precursor, as well as derivatives of the silicon-containing precursor. After the first precursor dose, the chamber is then evacuated to remove most or all of the first precursor that remains in the gas phase, leaving mostly or only the adsorbed species. In some implementations, the chamber may not be completely evacuated. For example, the reactor may be evacuated to a partial pressure of the first precursor in the gas phase low enough to slow the reaction. A second reactant (e.g., an oxygen-containing gas or a nitrogen-containing gas) is introduced into the chamber to cause some of its molecules to react with the first precursor adsorbed on the surface. In some processes, the second reactant reacts immediately with the adsorbed first precursor. In other embodiments, the second reactant reacts only when an activation source (e.g., plasma) is temporarily applied. The chamber can then be evacuated again to remove unbound second reactant molecules. As described above, in some embodiments, the chamber may not be completely evacuated. Additional ALD cycles may be used to build up film thickness.
[0062] exist Figure 3B In the example of , the n1 cycles are sufficient to deposit a thin liner layer within the one or more features to be filled with dielectric material. This layer will typically conform to the structure.
[0063] Although the n1 ALD cycles are typically thermal ALD cycles, there may be cases where PEALD is appropriate. In addition, the method can be used with other activation sources, such as exposure to UV light.
[0064] As shown above, in certain embodiments, ALD can be used to deposit silicon-containing films. Examples of silicon-containing reactants that can be used in the ALD method are further provided below. The method can also be used to form other dielectric films, which contain oxides such as gallium oxide, vanadium dioxide, hafnium oxide, zinc oxide, zirconium oxide, aluminum oxide, lithium (II) oxide, beryllium oxide, boron (III), magnesium oxide, titanium (III), iron (III), cobalt (II) oxide, and germanium (IV) oxide, as well as nitrides such as gallium nitride, aluminum nitride, lithium nitride, and boron nitride. Metals such as molybdenum, iron, cobalt, and germanium can be formed using these techniques, as well as compounds such as SiGe. Examples of reactants that can be used for these specific films are described below.
[0065] The second reactant (also referred to as a co-reactant) can vary depending on the film to be deposited. For example, oxygen (O2) can be used as a second reactant to deposit silicon and other oxides. Other second reactants can be used, including the use of other oxidants to deposit oxides, the use of nitrogen-containing reactants to deposit nitrides, the use of carbon-containing reactants to deposit carbides, etc. Examples include the use of O2 and / or nitrous oxide (N2O) to form a silicon oxide layer or a silicon oxynitride layer, the use of nitrogen (N2) or ammonia (NH3) to form a silicon nitride layer, the use of methane (CH4) to generate a silicon carbide layer, etc. A suitable mixture of reactants can be used to form carbon oxides, carbon nitride oxides, nitrogen oxides, carbon nitrides, etc.
[0066] After performing the n1 ALD cycles to deposit the liner film, a thermal inhibition process is performed. As described above, the thermal inhibition process involves exposure to a halogen-containing gas.
[0067] The thermal inhibition process may involve a continuous flow of the halogen-containing gas and other gases, if present. In certain embodiments, one or more of the gases flowing into the chamber may be pulsed. For example, the halogen-containing gas may be pulsed. If one or more additional gases are used, they may be continuously flowed and / or pulsed. Similarly, additional gases such as hydrogen and / or oxygen may be pulsed.
[0068] Back to Figure 3B, after performing the thermal inhibition process, performing n2 ALD cycles to deposit dielectric material, including in one or more features to be filled on the substrate. The reactants and deposited films in the ALD fill may be the same or different from the reactants used in the ALD liner operation and the deposited films formed. The number of cycles n2 is an integer of at least 1, and may be at least 2, at least 3, at least 4, at least 5, at least 6, at least 7, at least 8, at least 9, or at least 10. The number of cycles may depend on the structure geometry. For structures that are more challenging due to concavity, narrow openings, and / or high aspect ratios, fewer cycles may be used (thus having more inhibition and growth rate reduction). The thermal inhibition and the n2 ALD cycles may be repeated for n3 total cycles, where n3 is an integer of at least 1. (If any of n1, n2, or n3 is 1, the cycle under consideration is not repeated). In some embodiments, the total number of inhibition-fill cycles n3 is sufficient to complete the filling of one or more features. In some embodiments, the n2 used may be 2, 3, or 4. According to various embodiments, the number n2 may be constant during the process, or it may vary. For example, at the beginning of the fill process, the suppression may be more frequent. As features begin to fill from the bottom up or from the inside out, the filling may become less challenging, allowing for less frequent suppression.
[0069] After completing n3 thermal suppression-ALD fill cycles, further processing can be performed. This can include further ALD, PEALD, chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD) of dielectric materials, planarization, etching, etc.
[0070] Apart from Figure 1 In addition to the laterally oriented features in the example of FIG. 1 , this thermal suppression can also be used for other features that are difficult to suppress using plasma. These features include high aspect ratio features, including vertically oriented features with aspect ratios of 10:1 or greater.
[0071] In certain embodiments, the thermal inhibition can be used Figure 2 The concave features described. Since the thermal suppression process is conformal, it can be used to suppress deposition on the underside of the tip 215 and promote filling below. In some embodiments, thermal suppression can be used to fill structures whose surfaces may be damaged by plasma. For example, in a 3D NAND structure, a gap is formed by two stacks, each of which has multiple pairs of oxide layers and nitride layers. The stack can be capped with a polysilicon layer so that the polysilicon layer forms the sidewalls of the vertically oriented features to be filled. Plasma suppression treatment may damage the polysilicon layer. The thermal suppression process described herein can be used to perform damage-free gap filling from the inside out and from the bottom up.
[0072] As described above, the thermal inhibition involves exposure to halogen-containing gases. Examples of fluorine-containing gases include NF3, HF, fluorine (F2), carbon tetrafluoride (CF4), hexafluoroethane (C2F6), sulfur hexafluoride (SF6), chlorine trifluoride (ClF3), sulfur tetrafluoride (SF4), boron trifluoride (BF3), silicon tetrafluoride (SiF4), and difluorosilane (SiH2F4). Examples of chlorine-containing gases include hydrogen chloride (HCl), carbon tetrachloride (CCl4), thionyl chloride (SOCl2), chlorine (Cl2), boron trifluoride (BCl3), and silicon tetrafluoride (SiCl4). Examples of bromine-containing gases include bromine (Br2) and hydrobromic acid (HBr). Examples of iodine-containing gases include iodine (I2) and hydroiodic acid (HI).
[0073] Depending on the halogen-containing gas, one or more additional gases may be provided to promote the formation of the halogen-terminated surface. For example, H2O may be provided to react with the fluorine-containing gas to form HF, which may then form the F-terminated surface. In certain implementations, the halogen-containing gas is provided with a gas that forms water (e.g., H2 and O2). Other H-containing and / or O-containing compounds, such as H2O2, may be used. In certain implementations, the halogen-containing gas is provided with an organic solvent (e.g., alcohols) in addition to or in place of water.
[0074] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tertiary butanol, 1-pentanol, 1-hexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, and combinations thereof. In these or other cases, the organic solvent and / or water may include laboratory solvents. Examples of laboratory solvents include acetonitrile, methylene chloride, carbon tetrachloride, and combinations thereof. In these or other cases, the organic solvent and / or water may include ketones. Examples of ketones include acetone, acetophenone, and combinations thereof. In these or other implementations, the organic solvent and / or water may include alkanes. In certain embodiments, the alkanes may include alkanes selected from the group consisting of pentane, hexane, octane, cyclopentane, cyclohexane, and combinations thereof. In these or other embodiments, the organic solvent and / or water may include aromatic solvents. In some cases, the aromatic solvent is an aromatic solvent such as toluene and / or benzene. In these or other embodiments, the organic solvent and / or water may include ethers. In some such cases, the ethers may comprise tetrahydrofuran. In these or other implementations, the organic solvent and / or water may comprise nitriles. In some cases, the nitriles include acetonitrile. In these or other implementations, the organic solvent may comprise a carboxylic acid. In some cases, the carboxylic acid may include a carboxylic acid such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid and octanoic acid.
[0075] In certain embodiments, the halogen-containing gas may be provided without additional gas or with only an inert gas. Examples include halosilanes. These halosilanes may also be provided with additional gas.
[0076] The inhibition operation may be diffusion limited, where the depth of inhibition is controlled by one or more parameters such as inhibitor flow rate, inhibitor dilution, exposure time, and pressure. Figure 1 For example, in some embodiments, the suppression operation is performed so that the portion of each lateral directional feature 114 closest to the vertical directional hole 108 is suppressed, while the deeper portion of the lateral directional feature 114 is not suppressed or is suppressed to a lesser extent. In addition, as described above, the suppression degree of each lateral directional feature is the same from top to bottom.
[0077] According to various embodiments, the thermal inhibition processes described herein involve self-limiting etching of existing deposited materials. Figure 4 The thickness of a blanket SiO2 film deposited by ALD and subjected to thermal inhibition treatment at different pressures is shown. The upper line represents a pressure of 6 Torr, while the lower line represents a pressure of 17.5 Torr.
[0078] For both pressures, the thickness stabilizes after about 20 to 40 seconds. This indicates that the etch is self-limiting. Therefore, while pressure or other parameters can be used to ensure that the inhibition species reaches the appropriate portions of the structure, the etching and degree of inhibition of these portions are relatively insensitive to these parameters.
[0079] Figure 5 Shown is the subsequent ALD deposition thickness as a function of the number of ALD cycles after thermal inhibition of a blanket SiO2 film at 6 Torr and 17.5 Torr. The lines overlap perfectly, showing no pressure dependence. In this example, the inhibition time lasted for 2 to 3 cycles. Pressure may affect the degree of inhibition within a feature.
[0080] Even if the inhibition effect is still present, subsequent films may still grow at a slower growth rate because the inhibition treatment may not terminate every surface site where the precursor can adsorb.
[0081] Examples of chamber pressures include 0.2 to 760 Torr, such as 1 to 100 Torr or 1 to 30 Torr. In some embodiments, lower pressures (e.g., 0.2 to 10 Torr) may be used. Examples of substrate temperatures include 200°C to 950°C, such as 200°C to 800°C or 200°C to 750°C.
[0082] If the halogen-containing gas is mixed with other reactants and / or an inert carrier gas, it may be quite diluted. For example, 0.1 to 1 standard liter per minute (slm) of NF3, 5 slm of H2, and 5 slm of O2 may be used.
[0083] Another aspect of the present disclosure relates to using a plasma based suppression process to fill features. Figure 6 is a process flow diagram that depicts a method for filling a gap with a dielectric material. The method begins at operation 601, where a structure is provided, and the structure has one or more gaps to be filled. The structure can be formed by one or more material layers deposited on a substrate. The substrate can be a silicon or other semiconductor wafer, such as a 200 mm wafer, a 300 mm wafer, or a 450 mm wafer, including a wafer with one or more material layers (e.g., dielectric, conductive or semiconductor materials) deposited thereon. These methods can also be applied to gap filling of other substrates, such as glass, plastic, etc., including for the manufacture of microelectromechanical (MEMS) devices.
[0084] Examples of structures include VDRAM structures, 3D NAND structures, and shallow trench isolation (STI) structures. The structure includes multiple gaps, wherein the sidewalls of the gaps are formed by materials that are easily etched. In some embodiments, the structure may include a lateral structure extending horizontally from a common vertical trench. Examples of sidewall materials include nitrides, oxides, metals, and semiconductor materials. The methods described herein are not limited to a specific type of sidewall material and can be used to inhibit any material that is easily etched.
[0085] The dielectric material is deposited in the gap using a suppressed plasma (605). As discussed further below, this can involve atomic layer deposition (ALD) of the dielectric film followed by a cycle of suppressed plasma. According to various embodiments, exposure to the suppressed plasma can be performed at high pressure and / or high radical density.
[0086] To generate a plasma with a high radical density, an inductively coupled plasma (ICP) generator or a remote plasma generator may be used.
[0087] In some embodiments, a high pressure suppression plasma is used. High pressure refers to the pressure of the processing chamber during the suppression plasma process. In some embodiments, a capacitively coupled plasma (CCP) generator can be used to generate a high pressure plasma in situ in the processing chamber.
[0088] Using high pressure and / or high radical density plasma can provide a method for lateral gap filling structures (e.g. Figure 1) provides good top-down uniformity. In addition, in certain embodiments, halogen-free suppression materials can be used. As discussed further below, halogen-free suppression materials have various advantages, including preventing halogen incorporation into the film. However, they may be less effective in suppression. Using high pressure can improve the effectiveness of suppressing the plasma, especially for halogen-free suppression materials.
[0089] Figure 7 An example of a processing sequence that may be used in accordance with certain embodiments is shown. Figure 7 In an example processing sequence of , a substrate such as a semiconductor wafer is provided for gap filling. The substrate may be provided to a deposition chamber after prior processing and / or maintained in a deposition chamber. At this stage, the substrate includes one or more features to be filled with a dielectric material. For example, a substrate having Figure 1 A substrate with laterally oriented features is shown.
[0090] Next, n1 ALD deposition cycles are performed, where n1 is an integer of at least 1. As described above, an ALD cycle may include the following operations: (i) delivery / adsorption of a precursor, (ii) removal of the precursor from the chamber, (iii) delivery of a second reactant, and (iv) removal of byproducts from the chamber. The reaction between the second reactant and the adsorbed precursor to form a film on the substrate surface may affect the composition and properties of the film, such as non-uniformity, stress, wet etching rate, dry etching rate, electrical properties (e.g., breakdown voltage and leakage current), etc. In a plasma enhanced ALD (PEALD) process, a plasma may be ignited during or after the delivery of the second reactant in (iii). In reference to Figure 7 In the described method, either PEALD or thermal ALD can be used.
[0091] exist Figure 7 In the example of , the n1 cycles are sufficient to deposit a thin liner layer within the one or more features to be filled with dielectric material. The layer will typically conform to the structure.
[0092] The n1 ALD cycles can be thermal ALD or PEALD cycles. In addition, the method can be used with other activation sources, such as exposure to UV light.
[0093] As shown above, in certain embodiments, ALD can be used to deposit silicon-containing films. Examples of silicon-containing reactants that can be used in the ALD method are further provided below. The method can also be used to form other dielectric films, which contain oxides such as gallium oxide, vanadium dioxide, hafnium oxide, zinc oxide, zirconium oxide, aluminum oxide, lithium (II) oxide, beryllium oxide, boron (III), magnesium oxide, titanium (III), iron (III), cobalt (II) oxide, and germanium (IV) oxide, as well as nitrides such as gallium nitride, aluminum nitride, lithium nitride, and boron nitride. Metals such as molybdenum, iron, cobalt, and germanium can be formed using these techniques, as well as compounds such as SiGe. Examples of reactants that can be used for these specific films are described below.
[0094] The second reactant can vary depending on the film to be deposited. For example, oxygen (O2) can be used as a second reactant to deposit silicon and other oxides. Other second reactants can be used, including using other oxidants to deposit oxides, using nitrogen-containing reactants to deposit nitrides, using carbon-containing reactants to deposit carbides, etc. Examples include using O2 and / or nitrous oxide (N2O) to form a silicon oxide layer or a silicon oxynitride layer, using nitrogen (N2) or ammonia (NH3) to form a silicon nitride layer, using methane (CH4) to generate a silicon carbide layer, etc. A suitable reactant mixture can be used to form carbon oxides, carbon nitride oxides, nitrogen oxides, carbon nitrides, etc.
[0095] After performing the n1 ALD cycles to deposit the liner film, a plasma suppression process is performed.
[0096] In certain embodiments, the plasma suppression treatment involves exposing the liner film to a plasma containing a halogen plasma species, for example, the plasma may contain a halogen species, and the halogen species include anions and radical species, such as F-, Cl-, I-, Br-, fluorine radicals, etc. In some embodiments, the plasma is generated from a halogen-containing gas. Examples of fluorine-containing gases include NF3, HF, fluorine (F2), carbon tetrafluoride (CF4), hexafluoroethane (C2F6), sulfur hexafluoride (SF6), chlorine trifluoride (ClF3), sulfur tetrafluoride (SF4), boron trifluoride (BF3), silicon tetrafluoride (SiF4), and difluorosilane (SiH2F4). Examples of chlorine-containing gases include hydrogen chloride (HCl), carbon tetrachloride (CCl4), thionyl chloride (SOCl2), chlorine (Cl2), boron trifluoride (BCl3), and silicon tetrafluoride (SiCl4). Examples of bromine-containing gases include bromine (Br2) and hydrobromic acid (HBr). Examples of iodine-containing gases include iodine (I2) and hydroiodic acid (HI). In some embodiments, the inhibition produces an at least partially halogen-terminated surface.
[0097] Halogen-containing plasmas can be effective suppression plasmas. For example, in certain applications, plasmas generated from nitrogen trifluoride (NF3) can provide suppression effects in significantly less time than plasmas generated from molecular nitrogen (N2).
[0098] In some embodiments, a halogen-free suppression plasma is used. This can prevent halogens from being incorporated into the dielectric material. In addition to preventing halogens from being incorporated into the film, a nitrogen-containing and halogen-free suppression plasma (e.g., N2 plasma) can improve film properties by densifying the film. Another example of a nitrogen-containing and halogen-free plasma is a plasma produced by ammonia (NH3). In some embodiments, the nitrogen-containing and halogen-free suppression substance may include a plasma substance produced by amines, such as methylamine, dimethylamine, and trimethylamine. In some embodiments, the halogen-free substance may include a plasma substance produced by hydrazine (N2H4). In some embodiments, a nitrogen-containing compound may be provided together with hydrogen (H2). For example, a mixture of N2 and H2 may be used. The N2:H2 flow ratio may be from 1:1 to 75:1, such as 1:1, 10:1, 20:1, 50:1, and 75:1.
[0099] The suppression plasma treatment may result in over-suppression or under-suppression, which may result in insufficient deposition or voids, respectively. In certain embodiments, the suppression plasma treatment may be performed at high pressure. High pressure refers to the pressure of the processing chamber during the suppression plasma treatment. High pressure may increase the effectiveness of the suppression plasma, particularly for less effective suppressors, such as halogen-free suppressors, including halogen-free nitrogen-containing species, such as N2. In certain embodiments, the halogen-containing suppression plasma is at high pressure, thereby promoting uniformity of lateral gap fill from top to bottom.
[0100] Compared to low pressure suppressed plasma treatment, the duration of suppressed plasma treatment at high pressure can be significantly shortened without reducing the suppression depth, or even increasing the suppression depth. In certain embodiments, high pressure suppressed plasma treatment refers to a pressure greater than about 1 Torr, at least about 2 Torr, at least about 3 Torr, at least about 5 Torr, at least about 10 Torr, at least about 15 Torr, at least about 20 Torr, between about 10 Torr and 30 Torr, or between about 15 Torr and 30 Torr.
[0101] In some embodiments, the plasma can have a high radical density. For example, it can have more radical species than ionic species.
[0102] Back to Figure 7, after performing the suppression plasma treatment, performing n2 ALD cycles to deposit dielectric material, including in one or more features to be filled on the substrate. The reactants and deposited films in the ALD fill may be the same or different from the reactants used in the ALD liner operation and the deposited films formed. The number of cycles n2 is an integer of at least 1, and may be at least 2 or at least 3. In many embodiments, n2 is 1, with a suppression plasma performed with each ALD cycle. The number of cycles may depend on the geometry of the structure. For structures that are more challenging due to concavity, narrow openings, and / or high aspect ratios, fewer cycles may be used (thus with more suppression and a decrease in growth rate). The plasma suppression and the n2 ALD cycles may be repeated for n3 total cycles, where n3 is an integer of at least 1. (If any of n1, n2, or n3 is 1, the cycle under consideration is not repeated).
[0103] The sequence of inhibition followed by ALD may be referred to as an inhibition-deposition cycle. In certain embodiments, the total number of inhibition-deposition cycles n3 is sufficient to complete the filling of one or more features. In certain embodiments, n2 of 2, 3, or 4 may be used. According to various embodiments, the number of n2 may be constant during the process, or it may vary. For example, at the beginning of the fill process, the inhibition may be more frequent. As features begin to fill from the bottom up or from the inside out, the filling may become less challenging, allowing for less frequent inhibition.
[0104] After completing n3 inhibition-deposition cycles, further processing may be performed. This may include further ALD, PEALD, chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD) of dielectric materials, planarization, etching, etc.
[0105] Apart from Figure 1 In addition to the laterally oriented features in the example of FIG. 1 , the plasma suppression can also be used for other features that are difficult to suppress using plasma. These features include high aspect ratio features, including vertically oriented features with aspect ratios of 10:1 or more.
[0106] According to various embodiments, the chamber pressure during ALD and suppression plasma can be the same or different. In certain embodiments, the suppression plasma is relatively low power, for example, 2000 W for 4 stations (500 W for each station for a 300 mm wafer in a station) or less. In some embodiments, the power can be 1500 W for 4 stations (375 W for each station for a 300 mm wafer in a station) or less. Higher plasma powers do not tend to significantly increase the suppression effect.
[0107] During the PEALD operation, the plasma powers can be the same or different. Reducing the plasma power during PEALD will result in better suppression, but will have an adverse effect on film properties. In certain embodiments, the plasma power during PEALD can range from 3000W to 5000W for 4 stations (750W to 1250W for each station for a 300mm wafer in a station). In one example, the PEALD power for a 300mm wafer in a station is 1250W, followed by a 312.5W suppression process on the wafer. In these and other embodiments, the plasma power of the suppression plasma is lower than the plasma power of the PEALD.
[0108] The duration of suppression is an important factor in the degree of suppression. According to various embodiments, the duration of each suppression operation can be relatively long, for example from 5 seconds to 300 seconds. This duration can depend on the structure, with deeper structures using longer durations. In certain embodiments, the duration can be from 5 seconds to 20 seconds.
[0109] The chamber pressure can be constant throughout the process (including for ALD and suppressed plasma operations in the same chamber). An exemplary pressure range is from 5 Torr to 20 Torr. For PEALD and suppressed plasma, the chamber pressure can be less than 10 Torr, such as 6 Torr. For thermal ALD and suppressed plasma, the chamber pressure can vary, such as from 1 Torr to greater than 15 Torr.
[0110] An example of a substrate temperature is 500° C. to 700° C., such as 550° C. to 650° C. During the period of suppressing the plasma, the suppression effect increases as the temperature increases. Significantly lower temperatures (e.g., 50° C.) may also be used for suppression. In some embodiments, higher temperatures may be used to improve film properties if the thermal budget permits.
[0111] In certain embodiments, Figure 6 and Figure 7 The processing sequence shown in Figure 3A and Figure 3B The processing sequences shown in FIG. 1 and FIG. 2 are used in combination so that one or more suppression operations are thermal suppression operations and one or more suppression operations are plasma-based. Thermal suppression and plasma-based suppression can be performed in any order. For example, in certain embodiments, one or more cycles including thermal suppression can be used to deposit on sensitive underlying layers that may be damaged by exposure to plasma. After a certain thickness of film is deposited on the underlying layer, one or more cycles including plasma-based suppression can be used. Atomic Layer Deposition
[0112] Figure 8 A process flow diagram of a single ALD cycle is presented, wherein the single ALD cycle may be implemented as Figure 3B or Figure 7 , and a silicon-containing film is formed in the portion. In operation 802, the substrate is exposed to a silicon-containing precursor, thereby adsorbing the precursor to the surface of the feature. The operation can be self-limiting. In some embodiments, the precursor is not adsorbed on all active sites on the surface of the feature. In operation 804, the reaction chamber is optionally purged to remove the unadsorbed silicon-containing precursor. In operation 806, the substrate is exposed to a co-reactant. Examples thereof include O2 and / or N2O for forming a silicon oxide layer or a silicon oxynitride layer, N2 or NH3 for forming a silicon nitride layer, methane (CH4) for generating a silicon carbide layer, etc. For PEALD, the co-reactant can be a plasma species generated from a gas such as O2.
[0113] In operation 808, the reaction chamber is optionally purged to remove byproducts generated by the reaction between the silicon-containing precursor and the oxidant. Operations 802 to 808 are repeated for multiple cycles to deposit the silicon-containing layer in the feature to a desired thickness.
[0114] It should be noted that the treatments described herein are not limited to a particular reaction mechanism. Figure 8 The PEALD processes described include all deposition processes that use sequential exposure to silicon-containing reactants and conversion plasmas, including those that are not strictly self-limiting. The processes include sequences in which one or more gases used to generate the plasma flow continuously throughout the process, with intermittent plasma ignitions. For thermal inhibition, the processes include sequences in which one reactant (e.g., an oxidizing reactant) flows continuously while another reactant is pulsed.
[0115] Furthermore, while the description herein primarily relates to temporal ALD (wherein the substrate remains stationary in a particular environment, such as a chamber or workstation), the method may also be performed using spatial ALD. In spatial ALD, the substrate is moved to a different environment. Thus, according to various embodiments, the transition from operation 802 to operation 806 may include changing the chamber or workstation's susceptor temperature, chamber pressure, gas flow rate, etc., and / or moving the substrate to another chamber or workstation having different processing parameters.
[0116] In some embodiments of performing PEALD, the plasma is an in-situ plasma so that the plasma is directly formed above the substrate surface in the station. In some embodiments, the exemplary power / substrate area for the in-situ plasma of PEALD is between about 0.2122W / cm2 and about 2.122W / cm2. For example, for a chamber processing four 300mm wafers, its power range can be from about 1000W to about 6000W. In some embodiments, the power for four 300mm wafers can be between about 2500W and about 6000W. The plasma for ALD processing can be generated by applying a radio frequency (RF) field to the gas using two capacitive coupling plates. The ionization of the gas between the plates by the RF field ignites the plasma, thereby forming free electrons in the plasma discharge region. These electrons are accelerated by the RF field and can collide with gas phase reactant molecules. The collision of these electrons with reactant molecules can form free radical species participating in the deposition process. It should be understood that the RF field can be coupled via any suitable electrode. Non-limiting examples of electrodes include a treatment gas distribution showerhead and a substrate support pedestal. It should be understood that the plasma for the ALD process may be formed by one or more suitable methods other than capacitive coupling of the RF field to the gas. In one embodiment, the plasma is a remote plasma such that the second reactant is ignited in a remote plasma generator upstream of the station and then transported to the station housing the substrate.
[0117] ALD Reactants
[0118] For the deposition of silicon-containing films, one or more silicon-containing precursors may be used. According to the disclosed embodiments, suitable silicon-containing precursors include polysilane (H3Si-(SiH2)n-SiH3), where n>0. Examples of silanes include silane (SiH4), disilane (Si2H6) and organosilanes, such as methylsilane, ethylsilane, isopropylsilane, tert-butylsilane, dimethylsilane, diethylsilane, di(tert-butyl)silane, allylsilane, sec-butylsilane, tert-hexylsilane, isopentylsilane, tert-butyldisilane, di(tert-butyl)disilane, etc.
[0119] Halosilanes include at least one halogen group and may or may not include hydrogen and / or carbon groups. Examples of halosilanes are iodosilanes, bromosilanes, chlorosilanes and fluorosilanes. Specific chlorosilanes are tetrachlorosilane, trichlorosilane, dichlorosilane, monochlorosilane, chloroallylsilane, chloromethylsilane, dichloromethylsilane, chlorodimethylsilane, chloroethylsilane, tert-butylchlorosilane, di-tert-butylchlorosilane, chloroisopropylsilane, chloro-sec-butylsilane, tert-butyldiethylchlorosilane, n-hexyldimethylchlorosilane etc.
[0120] Aminosilanes contain at least one nitrogen atom bonded to a silicon atom, but may also contain hydrogen, oxygen, halogens, and carbon. Examples of aminosilanes are mono-, di-, tri-, and tetra-aminosilanes (H3Si(NH2), H2Si(NH2)2, HSi(NH2)3, and Si(NH2)4, respectively) and substituted mono-, di-, tri-, and tetra-aminosilanes, such as tert-butylaminosilane, methylaminosilane, tert-butylsilylamine, di(tert-butylamino)silane (SiH2(NHC(CH3)3)2(BTBAS), tert-butylsilylcarbamate, SiH(CH3)-(N(CH3)2)2, Si HCl-(N(CH3)2)2, (Si(CH3)2NH)3, di-isopropylaminosilane (DIPAS), di-sec-butylaminosilane (DSBAS), SiH2[N(CH2CH3)2]2(BDEAS), etc. A further example of an aminosilane is trisilylamine (N(SiH3)). In some embodiments, aminosilanes having two or more amine groups attached to the central silicon atom may be used. These may cause less damage than aminosilanes having only a single amine group attached.
[0121] Another example of a silicon-containing precursor includes trimethylsilane (3MS); ethylsilane; butylsilane; pentasilane; octylsilane; heptylsilane; hexasilane; cyclotetrasilane; cycloheptylsilane; cyclohexasilane; cyclooctylsilane; cyclopentasilane; 1,4-dioxa-2,3,5,6-tetrasilcyclohexane; diethoxymethylsilane (DEMS); diethoxysilane (DES); dimethoxymethylsilane; dimethoxysilane (DMOS); methyldiethoxysilane (MDES); methyldimethoxysilane (MDMS); octamethoxydodecyloxane (OMODDS); tert-butoxydisilane; tetramethylcyclotetrasiloxane (TMCTS); tetraoxymethylcyclotetrasiloxane (TOMCTS); triethoxysilane (TES); triethoxysiloxane (TRIES); and trimethoxysilane (TMS or TriMOS).
[0122] In certain embodiments, the silicon-containing precursor may include siloxane or siloxane containing amino groups. In certain embodiments, the siloxane used herein may have a chemical formula X(R 1 ) a Si-O-Si(R 2 ) b Y, wherein a and b are integers from 0 to 2, X and Y can independently be H or NR 3 R 4 , where R 1 , R 2 , R 3 , and R 4Each of X and Y is hydrogen, a linear alkyl group, a branched alkyl group, a saturated heterocyclic group, an unsaturated heterocyclic group, or a combination thereof. In certain embodiments, when at least one of X or Y is NR 3 R 4 When R 3 With R 4 Together with the atoms to which each of them is attached, a saturated heterocyclic compound is formed. In certain embodiments, the silicon-containing precursor is a pentamethylated siloxane containing an amino group, or a dimethylated siloxane containing an amino group. Examples of siloxanes containing amino groups include: 1-diethylamino 1,1,3,3,3,-pentamethyldisiloxane, 1-diisopropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-dipropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-di-n-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-di-sec-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-N-methylethylamino 1,1,3,3,3,-pentamethyldisiloxane disiloxane, 1-N-methylpropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1N-methylbutylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-tert-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-piperidinyl-1,1,3,3,3,-pentamethyldisiloxane, 1-dimethylamino-1,1-dimethyldisiloxane, 1-diethylamino-1,1-dimethyldisiloxane, 1-diisopropylamino-1,1-dimethyldisiloxane 1-dipropylamino-1,1-dimethyldisiloxane, 1-di-n-butylamino-1,1-dimethyldisiloxane, 1-di-sec-butylamino-1,1-dimethyldisiloxane, 1-N-methylethylamino-1,1-dimethyldisiloxane, 1-N-methylpropylamino-1,1-dimethyldisiloxane, 1-N-methylbutylamino-1,1-dimethyldisiloxane, 1-piperidinyl-1,1-dimethyldisiloxane, 1-tert-butylamino-1,1-dimethyldisiloxane, 1-dimethyl The invention discloses 1-amino-disiloxane, 1-di-n-butylamino-disiloxane, 1-di-sec-butylamino-disiloxane, 1-N-methylethylamino-disiloxane, 1-N-methylpropylamino-disiloxane, 1-N-methylbutylamino-disiloxane, 1-piperidinyl-disiloxane, 1-tert-butylamino-disiloxane, and 1-dimethylamino-1,1,5,5,5-pentamethyldisiloxane.
[0123] Examples of zirconium-containing precursors include bis(cyclopentadienyl)zirconium tetrahydride, bis(methyl-η5-cyclopentadienyl)methoxymethyl zirconium, dimethylbis(pentamethylcyclopentadienyl)zirconium(IV), tetrakis(diethylamide)zirconium(IV), tetrakis(diformamide)zirconium(IV), tetrakis(ethylmethylamide)zirconium(IV), bis(butoxy(bis-2,4-pentanedione)zirconium(IV), 2-ethylhexanoatezirconium(IV), and tetrakis(2,2,6,6-tetramethyl-3,5-heptanedione)zirconium.
[0124] Examples of hafnium-containing precursors include bis(tert-butylcyclopentadienyl)dimethyl hafnium(IV), bis(methyl-η5-cyclopentadienyl)dimethyl hafnium, bis(methyl-η5-cyclopentadienyl)methoxymethyl hafnium, bis(trimethylsilyl)amido hafnium(IV) chloride, dimethylbis(cyclopentadienyl) hafnium(IV), hafnium(IV) tert-butoxide, hafnium isopropoxide isopropanol adduct, tetrakis(diethylamido)hafnium(IV), tetrakis(dimethylamido)hafnium(IV), and tetrakis(ethylmethylamido)hafnium(IV).
[0125] Examples of vanadium-containing precursors include bis(cyclopentadienyl)vanadium(II) and vanadium(V)oxytriisopropoxide. An example of a niobium-containing precursor is bis(cyclopentadienyl)niobium(IV)dichloride. Examples of tantalum-containing precursors include penta(dimethylamino)tantalum(V), ethoxytantalum(V), tris(diacetamido)(tert-butylimino)tantalum(V), and tris(ethylmethylamido)(tert-butylimino)tantalum(V).
[0126] Examples of gallium-containing precursors include trimethylgallium and triethylgallium. Examples of aluminum-containing precursors include trimethylaluminum and aluminum chloride. Examples of zinc-containing precursors include zinc acetate, dimethylzinc, and diethylzinc.
[0127] In the case where the deposited film includes oxygen, an oxygen-containing reactant may be used. Examples of oxygen-containing reactants include, but are not limited to, oxygen (O2), ozone (O3), nitrous oxide (N2O), nitric oxide (NO), nitrogen dioxide (NO2), nitrogen trioxide (N2O3), nitrogen tetroxide (N2O4), nitrogen pentoxide (N2O5), carbon monoxide (CO), carbon dioxide (CO2), sulfur oxides (SO), sulfur dioxide (SO2), oxygenated hydrocarbons (C x H y O z ), water (H2O), formaldehyde (CH2O), carbonyl sulfide (COS), and mixtures thereof.
[0128] In the case where the deposited film contains nitrogen, a nitrogen-containing reactant may be used. The nitrogen-containing reactant contains at least one nitrogen, for example nitrogen (N2), ammonia (NH3), hydrazine (N2H4), such as methylamine (CH5N), dimethylamine ((CH3)2NH), ethylamine (C2H5NH2), isopropylamine (C3H9N), tert-butylamine (C4H 11 N), di(tert-butylamine)(C8H 19 N), cyclopropylamine (C3H5NH2), sec-butylamine (C4H 11 N), cyclobutylamine (C4H7NH2), isopentylamine (C5H 13 N), 2-methylbutan-2-amine (C5H 13 N), trimethylamine (C3H9N), diisopropylamine (C6H 15 N), diethylisopropylamine (C7H 17 N), di(tert-butyl)hydrazine (C8H 20 The nitrogen-containing reactants may include amines (e.g., amines with carbon) such as nitric acid (N2), and amines containing aromatic radicals such as aniline, pyridine, and benzylamine. The amines may be primary, secondary, tertiary, or quaternary (e.g., tetraalkylammonium compounds). In addition to nitrogen, the nitrogen-containing reactants may include heteroatoms such as hydroxylamine, tert-butyloxycarbonylamine, and N-tert-butylhydroxylamine. Other examples include nitrogen-containing reactants such as nitrous oxide (N2O), nitric oxide (NO), nitrogen dioxide (NO2), nitrogen trioxide (N2O3), nitrogen tetroxide (N2O4), and / or nitrogen pentoxide (N2O5). x O y Compound. Device
[0129] Fig. 9 A schematic diagram of an embodiment of an atomic layer deposition (ALD) processing station 900 is depicted, wherein the processing station 900 has a processing chamber body 902 for maintaining a low pressure environment. Multiple ALD processing stations 900 can be included in a common processing tool environment. For example, Fig.10 An embodiment of a multi-station processing tool 700 is depicted. In some embodiments, one or more hardware parameters of the ALD processing station 900 (including those discussed in detail herein) can be programmatically adjusted via one or more computer controllers 950.
[0130] The ALD processing station 900 is in fluid communication with a reactant delivery system 901a to deliver process gases to a distribution showerhead 906. The reactant delivery system 901a includes a mixing vessel 904 for mixing and / or conditioning process gases for delivery to the showerhead 906. In some embodiments, the inhibitor gas may be introduced into the mixing vessel before being introduced into the chamber body 902, for example if provided with a carrier gas. In some embodiments, the inhibitor or other gas may be delivered directly to the chamber body 902. One or more mixing vessel inlet valves 920 may control the introduction of process gases into the mixing vessel 904. The control of these valves may depend on whether the process gas, the inhibitory gas, or the carrier gas is adjusted to be open during various operations. In some embodiments, the inhibitory gas may be generated by using an inhibitory liquid and vaporizing it using a heated vaporizer.
[0131] For example, Fig. 9 Embodiments include a vaporization point 903, which is used to vaporize liquid reactants to be supplied to a mixing container 904. In some embodiments, the vaporization point 903 can be a heated vaporizer. The saturated reactant vapor produced from such a vaporizer will condense in the downstream delivery pipeline. Incompatible gases exposed to condensed reactants will produce small particles. These small particles may block pipelines, hinder valve operation, contaminate substrates, etc. Some methods for dealing with these problems involve cleaning and / or evacuating the delivery pipeline to remove residual reactants. However, cleaning the delivery pipeline will increase the processing station cycle time and reduce the processing station throughput. Therefore, in some embodiments, the delivery pipeline downstream of the vaporization point 903 can be heat traced. In some examples, the mixing container 904 can also be heat traced. In a non-limiting example, the pipeline downstream of the vaporization point 903 has a temperature profile that rises from about 100°C to about 150°C at the mixing container 904.
[0132] In some embodiments, a liquid precursor or reactant liquid (e.g., a silicon-containing precursor) may be vaporized at a liquid injector. For example, a liquid injector may inject a pulse of a liquid reactant into a carrier gas stream upstream of a mixing vessel. In one embodiment, a liquid injector may vaporize a reactant by flashing a liquid from a higher pressure to a lower pressure. In another example, a liquid injector may atomize a liquid into dispersed droplets that are then vaporized in a heated delivery pipe. Smaller droplets may vaporize faster than larger droplets, thereby reducing the delay between liquid injection and completion of vaporization. Faster vaporization may reduce the length of the pipeline downstream of vaporization point 603. In one case, a liquid injector may be loaded directly into a mixing vessel 604. In another case, a liquid injector may be loaded directly into a spray head 606.
[0133] In some embodiments, a liquid flow controller (LFC) (not shown) can be set upstream of the vaporization point 9603 to control the mass flow rate of the liquid for vaporization and delivery to the processing station 900. For example, the LFC can include a thermal mass flow meter (MFM) located downstream of the LFC. The plunger valve of the LFC can then be adjusted in response to a feedback control signal provided by a proportional integral differential (PID) controller that communicates electrically with the MFM. However, it can take one second or longer to use feedback control to stabilize the liquid flow. This can extend the time of dosing liquid reactants. Therefore, in some embodiments, the LFC can be dynamically switched between a feedback control mode and a direct control mode. In some embodiments, the LFC can be dynamically switched to a direct control mode from a feedback control mode by failing the sensing tube and the PID controller of the LFC.
[0134] The showerhead 906 distributes gas toward the substrate 912. For example, the showerhead 906 can distribute an inhibitor gas to the substrate 912, distribute a silicon-containing precursor to the substrate 912, or distribute a purge gas or a carrier gas to the chamber body 902, distribute a second reactant to the substrate 912, or distribute a passivation gas to the substrate 912 in various operations. Fig. 9 In the embodiment shown in , substrate 912 is positioned below showerhead 906 and is shown sitting on pedestal 908. Showerhead 906 can have any suitable shape and can have any suitable number and configuration of ports to distribute process gases to substrate 912.
[0135] In some embodiments, a microvolume is located below the showerhead 906. Implementing the disclosed embodiments in a microvolume rather than in the overall volume of the processing station can reduce reactant exposure and sweep time, can reduce the time to change processing conditions (e.g., pressure, temperature, etc.), can limit the exposure of the processing station robot to process gases, etc. Exemplary microvolume sizes include, but are not limited to, volumes between 0.1 liters and 2 liters. Such microvolumes can also have an impact on throughput. In some cases, the disclosed embodiments are not performed in a microvolume.
[0136] In some embodiments, the pedestal 908 can be raised or lowered to expose the substrate 912 to the microvolume 907 and / or to change the capacity of the microvolume 907. For example, during a substrate transfer phase, the pedestal 908 can be raised to position the substrate 912 within the microvolume 907. In some embodiments, the microvolume 907 can completely surround the substrate 912 and portions of the pedestal 908, thereby creating a high flow impedance region.
[0137] Optionally, the pedestal 908 can be lowered and / or raised during portions of the process to adjust the process pressure, reactant concentration, etc. within the microvolume 907. In one case where the process chamber body 902 is maintained at a base pressure during the process, lowering the pedestal 908 can allow the microvolume 907 to be evacuated. Exemplary ratios of microvolume to process chamber volume include, but are not limited to, volume ratios between 1:500 and 1:10. It should be understood that in some embodiments, the pedestal height can be programmatically adjusted by a suitable computer controller 950.
[0138] In another case, adjusting the height of the pedestal 908 can allow for changing the plasma density during an optional plasma activation process. For example, the plasma can be activated when a suppressant gas is introduced into the chamber body 902 or when a second reactant is flowed into the chamber body 902. In some embodiments, the plasma may not be activated during the flow of suppressant gas or the flow of the second reactant. At the end of this processing phase, the pedestal 908 can be lowered in another substrate transfer phase to allow the substrate 912 to be removed from the pedestal 908.
[0139] Although the exemplary microvolume variations described herein relate to a height-adjustable pedestal 908, it should be understood that in some embodiments, the position of the showerhead 906 can be adjusted relative to the pedestal 908 to change the volume of the microvolume 907. In addition, it should be understood that the vertical position of the pedestal 908 and / or showerhead 906 can be changed by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 908 may include a rotation axis for rotating the orientation of the substrate 912. It should be understood that in some embodiments, one or more of these exemplary adjustments can be performed programmatically by one or more appropriate controllers 950.
[0140] If plasma is used (e.g., for PEALD), the showerhead 906 and the pedestal 908 are electrically connected to a radio frequency (RF) power source 914 and a matching network 916 to power the plasma. In some embodiments, the plasma energy can be controlled by controlling one or more of the processing station pressure, gas concentration and gas partial pressure or gas flow rate, RF source power, RF source frequency, and plasma power pulse timing. For example, the RF power source 914 and the matching network 916 can be operated at any suitable power to form a plasma with a component of a desired free radical species. Examples of suitable power are included above. Similarly, the RF power source 914 can provide RF power of any appropriate frequency. In some embodiments, the RF power source 914 can be configured to control a high frequency RF power source and a low frequency RF power source that are independent of each other. Exemplary low frequency RF frequencies may include, but are not limited to, frequencies between 0kHz and 500kHz. Exemplary high frequency RF frequencies may include, but are not limited to, frequencies between 1.8 MHz and 2.45 GHz, or above about 13.56 MHz, or above 27 MHz, or above 40 MHz, or above 60 MHz. It should be appreciated that any suitable parameter may be discretely or continuously adjusted to provide plasma energy for surface reactions. In a non-limiting example, the plasma power may be intermittently pulsed to reduce ion bombardment of the substrate surface relative to a continuously powered plasma.
[0141] In some embodiments, the plasma can be monitored in situ by one or more plasma monitors. In one case, the plasma power can be monitored by one or more voltage and current sensors (e.g., VI probes). In another case, the plasma density and / or the concentration of the process gas can be measured by one or more optical emission spectrometer sensors (OES). In some embodiments, one or more plasma parameters can be adjusted programmatically based on the measurement results from such an in-situ plasma monitor. For example, an OES sensor can be used in a feedback loop to provide programmatic control of the plasma power. It should be understood that in some embodiments, other monitors can be used to monitor plasma and other processing characteristics. Such monitors may include, but are not limited to, infrared (IR) monitors, acoustic monitors, and pressure sensors.
[0142] In some embodiments, the instructions used by the controller 950 may be provided via input / output control (IOC) sequence instructions. In one example, instructions for setting the conditions used in the processing stage may be included in the corresponding recipe stage of the processing recipe. In some cases, the processing recipe stages may be arranged in sequence so that all instructions for the processing stage are executed simultaneously with the processing stage. In some embodiments, instructions for setting one or more reactor parameters may be included in the recipe stage. For example, a first recipe stage may include instructions for setting the flow rate of an inert gas and / or a reactant gas (e.g., a first reactant, such as a silicon-containing precursor), instructions for setting the flow rate of a carrier gas (e.g., argon), and time delay instructions for the first recipe stage. A subsequent second recipe stage may include instructions for adjusting or stopping the flow rate of an inert gas and / or a reactant gas, instructions for adjusting the flow rate of a carrier gas or a purge gas, and time delay instructions for the second recipe stage. The third recipe stage may include instructions for setting the flow rate of the inert gas, inhibitor gas, and / or reactant gas (which may be the same or different from the gas used in the first recipe stage), instructions for adjusting the flow rate of the carrier gas, and time delay instructions for the third recipe stage. The fourth recipe stage may include instructions for adjusting or stopping the flow rate of the inert gas and / or reactant gas (e.g., a second reactant such as nitrogen or a nitrogen-containing gas or an oxygen-containing gas), instructions for adjusting the flow rate of the carrier gas or purge gas, and time delay instructions for the fourth recipe stage. It should be understood that these recipe stages may be further subdivided and / or repeated in any suitable manner within the scope of the present disclosure.
[0143] In some embodiments, the pedestal 908 can be temperature controlled by the heater 610. In addition, in some embodiments, pressure control of the processing station 900 can be provided by a butterfly valve 918. Fig. 9 In the embodiment shown in FIG. 1 , butterfly valve 918 throttles the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, the pressure control of the process station 900 can also be adjusted by changing the flow rate of one or more gases introduced into the process station 900.
[0144] As described above, one or more processing stations may be included in a multi-station processing tool. Fig.10A schematic diagram showing an embodiment of a multi-station processing tool 1000 having an inbound load lock 1002 and an outbound load lock 704, one or both of which may include a remote plasma source. A robot 1006 at atmospheric pressure is configured to move a wafer from a wafer cassette to the inbound load lock 902. The wafer is placed on a pedestal 1012 in the inbound load lock 1002 by the robot 1006, the atmospheric port 1010 is closed and the load lock is evacuated. In the case where the inbound load lock 1002 includes a remote plasma source, the wafer may be exposed to a remote plasma treatment in the load lock before being directed into a processing chamber 1014. In addition, the substrate may also be heated in the inbound load lock 1002 to, for example, remove moisture and adsorbed gases. Next, the chamber transfer port 1016 to the process chamber 1014 is opened and the robot places the wafer into the reactor and onto the susceptor at the first station shown in the reactor for processing. Fig.10 The embodiments depicted in include a load lock, but it will be appreciated that in some embodiments, wafers may be provided directly into a processing station.
[0145] The depicted processing chamber 1014 includes four processing stations, numbered 1 to 4 in the embodiment shown in Figure 19. Each station has a heated susceptor (shown as 1018 for station 1) and a gas pipeline inlet. It should be understood that in some embodiments, each processing station can be used for different or multiple purposes. Although the depicted processing chamber 1014 includes four stations, it should be understood that processing chambers according to the present invention can have any suitable number of stations. For example, in some embodiments, the processing chamber can have five or more stations, while in other embodiments, the processing chamber can have three or fewer stations.
[0146] Each station may perform the same or different operations as another station.In some embodiments, suppression is performed only in one or a subset of the stations.
[0147] Fig.10 An embodiment of a wafer handling system 1090 for transferring wafers is depicted. In some embodiments, the wafer handling system 1090 can transfer wafers between various processing stations and / or between a processing station and a load lock. It should be understood that any suitable wafer handling system can be employed. Non-limiting examples include wafer carousels and wafer handling robots. Fig.10Also depicted is an embodiment of a system controller 1050 for controlling processing conditions and hardware states of the processing tool 1000. The system controller 1050 may include one or more memory devices 1056, one or more mass storage devices 1054, and one or more processors 1052. The processor 1052 may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, and the like.
[0148] In some embodiments, the system controller 1050 controls all activities of the processing tool 1000. The system controller 1050 executes system control software 1058 stored in the mass storage device 1054, loaded into the storage device 1056 and executed on the processor 1052. Alternatively, the control logic can be hard-coded in the controller 1050. Application-specific integrated circuits, programmable logic devices (such as field programmable gate arrays or FPGAs), etc. can be used for these purposes. In the following discussion, wherever "software" or "coding" is used, functionally comparable hard-coded logic can be used therein. The system control software 1058 can include parameters for controlling timing, gas mixtures, gas flow rates, chamber and / or station pressures, chamber and / or station temperatures, wafer temperatures, target power levels, RF power levels, substrate pedestals, chucks and / or sensor positions, and other parameters for specific processes performed by the processing tool 1000. The system control software 1058 can be configured in any suitable manner. For example, various processing tool component subroutines or control objects can be written to control the operation of processing tool components used to perform various processing tool processes. The system control software 1058 may be coded in any suitable computer readable programming language.
[0149] In some embodiments, the system control software 1058 may include input / output control (IOC) sequencing instructions for controlling the various parameters described above. In some embodiments, other computer software and / or programs stored on the mass storage device 1054 and / or the memory device 856 associated with the system controller 1050 may be used. Examples of programs or portions of programs for this purpose include substrate positioning programs, process gas control programs, pressure control programs, heater control programs, and plasma control programs.
[0150] The substrate positioning program may include program code used by process tool components for loading a substrate onto the pedestal 1018 and controlling the spacing between the substrate and other components of the process tool 1000 .
[0151] The process gas control program may include code for controlling gas composition (e.g., silicon-containing precursors, co-reactants, inhibition gases, passivation gases, and sweep gases as described herein) and flow rates, and optionally for flowing gases into one or more process stations to stabilize the pressure within the process station prior to deposition. The pressure control program may include code for controlling the pressure within the process station, for example, by adjusting a throttle valve within the exhaust system of the process station, gas flow into the process station, etc.
[0152] The heater control program may include code for controlling the flow of current to a heating unit that is used to heat the substrate. Alternatively, the heater control program may control the delivery of a heat transfer gas (eg, helium) toward the wafer.
[0153] A plasma control program may include code for setting RF power levels applied to process electrodes within one or more process stations in accordance with embodiments herein.
[0154] The pressure control program may include code for maintaining the pressure within a reaction chamber according to embodiments herein.
[0155] In some embodiments, there may be a user interface associated with the system controller 1050. The user interface may include a display screen, a graphical software display of apparatus and / or processing conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, etc.
[0156] In some embodiments, the parameters adjusted by the system controller 1050 may be related to process conditions. Non-limiting examples include composition and flow rate of process gases, temperature, pressure, plasma conditions (e.g., RF bias power level), etc. These parameters may be provided to the user in the form of a recipe that may be input using a user interface.
[0157] A number of signals used to monitor the process may be provided from sensors of various process tools through analog and / or digital input connections of the system controller 1050. Signals used to control the process may be output through analog and digital output connections of the process tool 1000. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (e.g., manometers), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with the data from these sensors to maintain process conditions.
[0158] The controller 1050 may provide program instructions for implementing the above-described deposition process. The program instructions may control various process parameters, such as DC power level, RF bias power level, pressure, temperature, etc. The instructions may control these parameters to operate the in-situ deposition of the film stack according to the various embodiments described herein.
[0159] The system controller 1050 will typically include one or more memory devices and one or more processors configured to execute instructions so that the apparatus will perform the method according to the present embodiment. A machine-readable medium containing instructions for controlling processing operations according to the present embodiment may be coupled to the system controller 1050.
[0160] In some implementations, the system controller 1050 is part of a system, which can be part of the above examples. Such a system can include a semiconductor processing device, which includes one or more processing tools, one or more chambers, one or more platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems can be integrated with electronic devices for controlling their operation before, during, and after the processing of semiconductor wafers or substrates. The electronic device can be referred to as a "controller", which can control various components or subcomponents of one or more systems. Depending on the processing conditions and / or system type, the system controller 1050 can be programmed to control any of the processes disclosed herein, including the delivery of process gases and / or inhibitor gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer in and out of tools connected or docked with specific systems and other transfer tools and / or load locks.
[0161] In general, the system controller 1050 may be defined as an electronic device having various integrated circuits, logic, memory, and / or software to receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, and the like. The integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions may be instructions sent to the system controller 1050 in the form of various individual settings (or program files) that define operating parameters for performing a particular process on or for a semiconductor wafer or system. In some embodiments, the operating parameters may be part of a recipe defined by a process engineer to accomplish one or more process steps during the manufacture of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.
[0162] In some implementations, the system controller 1050 may be part of or coupled to a computer that is integrated with the system, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the system controller 1050 may be in the "cloud" or may be all or part of a wafer fab host system that may allow remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance criteria for multiple manufacturing operations, to change parameters of a current process, set processing steps to follow a current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a processing recipe to the system over a network (which may include a local network or the Internet). The remote computer may include a user interface that enables input or programming of parameters and / or settings, which are then sent from the remote computer to the system. In some examples, the system controller 750 receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. The parameters may be specific to the type of process to be performed and the type of tool that the system controller 1050 is configured to interface with or control. Thus, as described above, the system controller 1050 can be distributed, for example, by including one or more discrete controllers networked together and working toward a common purpose (e.g., processing and control as described herein). An example of a distributed controller for such a purpose is one or more integrated circuits on a chamber that communicate with one or more integrated circuits remotely (e.g., at a platform level or as part of a remote computer), which combine to control processing on the chamber.
[0163] Exemplary systems may include, but are not limited to, plasma etching chambers or modules, deposition chambers or modules, spin rinse chambers or modules, metal plating chambers or modules, cleaning chambers or modules, chamfer edge etching chambers or modules, physical vapor deposition (PVD) chambers or modules, chemical vapor deposition (CVD) chambers or modules, ALD chambers or modules, atomic layer etching (ALE) chambers or modules, ion implantation chambers or modules, track chambers or modules, and any other semiconductor processing system that may be associated with or used in the manufacture and / or preparation of semiconductor wafers.
[0164] As described above, depending on one or more processing steps to be performed by the tool, the system controller 1050 can communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a host computer, another controller, or tools used in the transport of materials for transporting wafer containers to and from tool locations and / or load ports in a semiconductor manufacturing facility.
[0165] Fig.11Block diagram of another processing system suitable for performing deposition processing according to certain embodiments. System 1100 includes a transport module 1103. Mounted on transport module 1103 are two multi-station reactors 1109 and 1110, each of which is capable of performing inhibition processing and / or ALD and / or CVD according to certain embodiments. Reactors 1109 and 1110 may include multiple stations 1111, 1113, 1115, and 1117, and these stations may perform operations according to the disclosed embodiments in sequence or non-sequentially. The stations may include a heated pedestal or substrate support, one or more gas inlets, showerheads, or diffuser plates.
[0166] Also mounted on the transfer module 1103 may be one or more single or multi-station modules 1107 capable of performing plasma or chemical (non-plasma) pre-cleaning, or any other processing related to the disclosed methods. In some cases, module 1107 may be used for a variety of processing, such as preparing a substrate for a deposition process. Module 1107 may also be designed / configured to perform a variety of other processing, such as etching or polishing. The system 1100 also includes one or more wafer source modules 1101, where wafers are stored before and after processing. An atmospheric robot (not shown) in the atmospheric transfer chamber 1119 may first move the wafer from the source module 1101 to the load lock 1121. The wafer transfer equipment (typically a robot arm unit) in the transfer module 1103 moves the wafer from the load lock 1121 to modules mounted on the transfer module 1103 and to modules mounted on the transfer module 1103. In various embodiments, the system controller 1129 is used to control the movement of wafers from the source module 1101 to the load lock 1121. Fig.10 The processing conditions during deposition are described above.
[0167] The system control logic used for the system controller described herein can be configured in any suitable manner. In general, the logic can be designed or configured in hardware and / or software. The instructions for controlling the drive circuit can be hard-coded or provided as software. The instructions can be provided by "programming". Such programming is understood to include any form of logic, including hard-coded logic in digital signal processors, application-specific integrated circuits, and other devices with specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions that can be executed on a general-purpose processor. The system control software can be encoded in any suitable computer-readable programming language.
[0168] The computer program code for controlling the germanium-containing reducing agent pulses, hydrogen gas flow, and tungsten-containing precursor pulses, as well as other processes in the process sequence, can be written in any commonly used computer-readable programming language: for example, assembly language, C, C++, Pascal, Fortran, or others. The compiled object code or script is executed by the processor to perform the tasks identified in the program. Also as indicated, the program code can be hard-coded.
[0169] Controller parameters relate to process conditions such as, for example, process gas composition and flow rate, temperature, pressure, cooling gas pressure, substrate temperature, and chamber wall temperature. These parameters are provided to the user in the form of recipes and can be input using a user interface. Signals for monitoring the process can be provided via analog and / or digital input connections of the system controller 950 or 1050. Signals for controlling the process are output via analog and digital output connections of the deposition apparatus.
[0170] The system software may be designed or configured in many different ways. For example, various chamber component subroutines or control objects may be written to control the operation of chamber components necessary to perform deposition processes (and in some cases other processes) in accordance with the disclosed embodiments. Examples of programs or program segments for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.
[0171] In some implementations, a controller (e.g., controller 950, 1050, or 1129) is part of a system, which can be part of the above examples. Such a system can include a semiconductor processing device, which includes one or more processing tools, one or more chambers, one or more platforms for processing, and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems can be integrated with electronic devices for controlling their operation before, during, and after processing of semiconductor wafers or substrates. The electronic device can be referred to as a "controller", which can control various components or subcomponents of one or more systems. Depending on the processing requirements and / or the type of system, the controller can be programmed to control any of the processes disclosed herein, including the delivery of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer in and out of tools connected or docked with specific systems and other transfer tools and / or load locks.
[0172] In general, a controller can be defined as an electronic device having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuit can include a chip in the form of firmware that stores program instructions, a digital signal processor (DSP), a chip defined as an application specific integrated circuit (ASIC), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions can be instructions sent to the controller in the form of various individual settings (or program files) that define operating parameters for performing specific processing on or for a semiconductor wafer or system. In some embodiments, the operating parameters can be part of a recipe defined by a process engineer to complete one or more processing steps during the manufacture of one or more (kinds of) layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.
[0173] In some implementations, the controller may be part of or coupled to a computer that is integrated with the system, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the controller may be in the "cloud" or may be all or part of a wafer fab host system that may allow remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, check the history of past manufacturing operations, check trends or performance criteria for multiple manufacturing operations, to change the parameters of the current processing, set processing steps to follow the current processing, or start a new processing. In some examples, a remote computer (e.g., a server) may provide a processing recipe to the system via a network (which may include a local network or the Internet). The remote computer may include a user interface that enables input or programming of parameters and / or settings, which are then sent from the remote computer to the system. In some examples, the controller receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. It should be understood that the parameters may be specific to the type of processing to be performed and the type of tool that the controller is configured to interface with or control. Thus, as described above, the controller may be distributed, for example, by including one or more discrete controllers networked together and working toward a common purpose (e.g., processing and control as described herein). An example of a distributed controller for such a purpose is one or more integrated circuits on a chamber that communicate with one or more integrated circuits remotely (e.g., at a platform level or as part of a remote computer), which combine to control processing on the chamber.
[0174] Exemplary systems may include, but are not limited to, plasma etching chambers or modules, deposition chambers or modules, spin rinse chambers or modules, metal plating chambers or modules, cleaning chambers or modules, chamfer edge etching chambers or modules, physical vapor deposition (PVD) chambers or modules, chemical vapor deposition (CVD) chambers or modules, atomic layer deposition (ALD) chambers or modules, atomic layer etching (ALE) chambers or modules, ion implantation chambers or modules, track chambers or modules, and any other semiconductor processing system that may be associated with or used in the manufacture and / or preparation of semiconductor wafers.
[0175] As described above, depending on one or more processing steps to be performed by the tool, the controller can communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a host computer, another controller, or tools used in material transport to transport wafer containers to and from tool locations and / or load ports in a semiconductor manufacturing facility.
[0176] It should be understood that multiple processing stations may be included in a multi-station processing tool environment, such as Fig.12 , which depicts a schematic diagram of an embodiment of a multi-station processing tool. Processing equipment 1200 uses an integrated circuit fabrication chamber 1263 that includes a plurality of fabrication processing stations, each of which can be used to perform processing operations on a substrate supported in a substrate support (e.g., a susceptor) at a particular processing station. Fig.12 In the embodiment of the present invention, the integrated circuit fabrication chamber 1263 is shown as having four processing stations 1251, 1252, 1253 and 1254. Other similar multi-station processing equipment may have more or fewer processing stations depending on the implementation and, for example, the desired degree of parallel wafer processing, size / space constraints, cost constraints, etc. Fig.12 Also visible is a substrate handling robot 1275, which can be operated under the control of a system controller 1290 to transfer a substrate from a wafer cassette (not shown). Fig.12 Multiple substrates (in the embodiment of the present invention) are moved from the loading port 1280 into the integrated circuit manufacturing chamber 1263 and moved to one of the processing stations 1251, 1252, 1253 and 1254.
[0177] Fig.12 Also shown is one implementation of a system controller 1290 for handling processing conditions and hardware states of the apparatus 1200. As described herein, the system controller 1290 may include one or more memory devices, one or more mass storage devices, and one or more processors.
[0178] RF subsystem 1295 can generate RF power and transmit RF power to integrated circuit fabrication chamber 1263 through RF input port 1267. In certain embodiments, integrated circuit fabrication chamber 1263 may include input ports in addition to RF input port 1267 (additional input ports are not shown). Fig.12 ). Thus, eight RF input ports may be used by the integrated circuit fabrication chamber 1263. In a particular embodiment, each of the processing stations 1251-1254 in the integrated circuit fabrication chamber 1263 may use a first and a second input port, wherein the first input port may transmit a signal having a first frequency and the second input port may transmit a signal having a second frequency. Using dual frequencies may provide enhanced plasma characteristics.
[0179] According to various embodiments, the suppression and deposition operations of each cycle can be performed in the same or different chambers. In some embodiments, the suppression and deposition operations are performed in a chamber with appropriate control of gas flow and RF power as described above for each operation. In a multi-station chamber, one or more stations can be used for deposition and one or more different stations can be used for suppression. Alternatively, each station can be used for both operations.
[0180] The apparatus / processes described herein can be used in conjunction with photolithographic patterning tools or processes, e.g., for preparing or manufacturing semiconductor devices, displays, LEDs, photovoltaic panels, etc. Typically, though not necessarily, these tools / processes will be used or operated together in a common manufacturing facility. Photolithographic patterning of films typically involves some or all of the following operations, each of which enables multiple available tools: (1) applying photoresist on a workpiece (i.e., substrate) using a spin coating or spray coating tool; (2) curing the photoresist using a hot plate or oven or UV curing tool; (3) exposing the photoresist to visible light or ultraviolet light or x-rays using a tool such as a wafer stepper; (4) developing the resist to selectively remove the resist and thereby pattern it using a tool such as a wet bench; (5) transferring the resist pattern to an underlying film or workpiece by using a dry or plasma assisted etching tool; and (6) removing the resist using a tool such as an RF or microwave plasma resist stripper. in conclusion
[0181] Although the above embodiments have been described in some detail for the purpose of clarity of understanding, it is apparent that certain variations and modifications may be implemented within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, systems and devices of the embodiments of the present invention. Therefore, the embodiments of the present invention should be considered illustrative rather than restrictive, and the embodiments are not limited to the details given herein.
Claims
1. A method of filling a feature of a structure on a substrate in a chamber, comprising: Perform one or more cycles of the following steps: (e) providing a halogen-containing gas to the chamber in the absence of a plasma to inhibit deposition on at least a portion of the feature; (f) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
2. The method according to claim 1, wherein: The dielectric material is oxide, nitride or carbide. 3 . The method of claim 1 , further comprising, prior to performing one or more cycles of (a) and (b), depositing a liner layer in the feature by atomic layer deposition.
4. The method according to claim 1, wherein: (a) Leads to self-limiting etching.
5. The method according to claim 1, wherein: (a) Production of halogen-terminated surfaces.
6. The method according to claim 1, wherein: (a) further comprises providing water, or one or more reactants capable of forming water, to the chamber.
7. The method according to claim 1, wherein: (b) includes providing a halogen-containing gas, hydrogen (H2) and oxygen (O2) to the chamber.
8. The method according to claim 1, wherein: The structure includes a vertically oriented feature having a sidewall, a plurality of openings in the sidewall creating a plurality of laterally oriented features fluidly accessible through the plurality of openings, wherein the feature is one of the laterally oriented features.
9. The method of claim 8, further comprising performing one or more cycles of the following steps: (g) providing a halogen-containing gas or a halogen-free gas to the chamber under plasma conditions to inhibit deposition on at least a portion of the feature; (h) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
10. A method of filling a feature of a structure on a substrate in a chamber, comprising: Perform one or more inhibition-deposition cycles of the following steps: (c) providing a plasma generated from a nitrogen-containing, halogen-free gas to the chamber to inhibit deposition on at least a portion of the feature, wherein during (a), the pressure of the chamber is at least 5 Torr; and (d) performing one or more atomic layer deposition cycles to deposit a dielectric material in the feature.
Citation Information
Cited By
Atomic layer deposition process and structure for forming air gap