Preparation method of composite carbon nanotube functional filtering membrane
By adding surfactant and binder to the carbon nanotube composite membrane, and using titanium dioxide or iron oxide as intercalation substances, a functional filter membrane of composite carbon nanotubes was prepared by spraying, the low dye removal rate in the prior art was solved. and the problem of poor mechanical properties, efficient dye separation and sewage treatment are achieved.
Patent Information
- Application Number
- CN202411376528.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The existing carbon nanotube composite membranes have low removal rate during dye filtration and have poor mechanical properties, making it difficult to effectively separate dye solutions in a short period of time.
The composite film is prepared by hot pressing the PTFE microporous film and PET nonwoven material. The activated carbon nanotubes are uniformly mixed with surfactant and adhesive, combined with titanium dioxide or iron oxide as rigid intercalation substances, and spraying method is used. A composite carbon nanotube functional filter membrane with layer-layer assembly structure was prepared.
It realizes efficient dye solution separation, improves the hydrophilicity and filtration efficiency of the membrane, enhances the sewage treatment capacity, simplifies the manufacturing process, reduces production costs, and improves the tolerance and production efficiency of the equipment.
Smart Images

Figure CN119056264A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional membrane material preparation, and in particular relates to a method for preparing a composite carbon nanotube functional filter membrane with a layer-by-layer assembly structure. Background Art
[0002] Membrane separation technology is a new separation technology developed based on the intersection of multiple disciplines such as materials science and engineering. Due to its unique advantages and performance, it has attracted much attention in scientific research and industrial applications. At present, membrane separation technology is in the field of water treatment applications. It can effectively cope with the high filtration water quality requirements that are difficult to meet with traditional water treatment technologies, and more efficiently solve water environmental pollution problems. However, with the development of science and technology, single-function membrane separation technology has been unable to meet technical needs.
[0003] Carbon nanotubes were discovered by Lijima on the cathode surface in the arc discharge method in 1991. The carbon nanotube film constructed by them has an adjustable microstructure surface, high mechanical strength, good mechanical, electrical and adsorption properties, and a long service life. It can be recycled and reused. It has been widely studied in recent years and has been widely used in dye filtration, oil-water separation, composite materials and other fields.
[0004] Patent CN107602927A discloses a method for preparing and applying a carbon nanotube composite membrane, wherein cellulose, carbon nanotubes and poly (N-isopropylacrylamide) gel nanospheres are blended with ionic liquid to prepare a near-infrared laser responsive composite membrane material, which can be applied to the control of dye concentration in textile printing and dyeing. The carbon nanotube composite membrane prepared by this method has a small difference in absorbance for the dye solution, indicating that the carbon nanotube membrane has a low removal rate for the dye.
[0005] Patent CN116550317A discloses a method for preparing a multi-scale titanium dioxide fiber / carbon nanotube film composite photocatalyst, which mainly uses microemulsion electrospinning to prepare TiO2 fibers on the surface of a carbon nanotube array while drawing it, thereby obtaining the multi-scale TiO2 fiber / carbon nanotube film. This method can effectively solve the problem of poor mechanical properties of the carbon nanotube film. It can be seen from the results after photocatalysis that the film needs to reach a certain time before the adsorption of the dye solution can be effectively carried out. The present invention improves on this feature of efficient dye filtration to obtain a composite carbon nanotube functional filtration membrane that effectively separates the dye solution in a short time. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a composite carbon nanotube functional filtration membrane with good hydrophilicity.
[0007] In order to solve the above problems, the present invention provides a method for preparing a composite carbon nanotube functional filtration membrane, comprising the following steps:
[0008] 1) Preparation of organic membrane support:
[0009] The PTFE microporous membrane (pore size 0.45 μm) and the PET nonwoven material were hot pressed to prepare a composite membrane;
[0010] 2) Preparation of carbon nanotube composite liquid:
[0011] After the carbon nanotube powder is activated, a surfactant is added and uniformly mixed (ultrasonic oscillation is performed after uniform stirring, and the ultrasonic oscillation time is 30 to 90 minutes) to obtain a carbon nanotube / surfactant mixed solution; a binder is added to the carbon nanotube / surfactant mixed solution and uniformly mixed (mechanical stirring for 10 to 20 minutes, ultrasonic oscillation for 20 to 40 minutes; "mechanical stirring-ultrasonic oscillation" is performed 2 to 4 times in total) to obtain a carbon nanotube composite liquid (uniformly dispersed carbon nanotube composite liquid); the mass ratio of the carbon nanotube to the surfactant is 1:1 to 2, and the volume ratio of the binder to the carbon nanotube / surfactant mixed solution is 2:3 to 4;
[0012] 3) Preparation of titanium dioxide as a rigid intercalation material:
[0013] The titanium tetrachloride is hydrolyzed and centrifuged to obtain a precipitate, the precipitate is washed with water, and then dried and calcined in sequence to obtain titanium dioxide (titanium dioxide particles);
[0014] 4) Preparation of iron oxide as a rigid intercalation material:
[0015] The ferric chloride is placed in a reaction kettle and subjected to a hydrothermal reaction under the action of a reducing agent. The temperature of the hydrothermal reaction is in the range of 140 to 240° C. and the time is 10 to 18 hours. After the reaction is completed, the reaction is centrifuged (7000 to 10000 rpm, 25 to 55 minutes), and the precipitate obtained by centrifugation is washed with water to obtain a precursor FeCO3. The reducing agent is ascorbic acid or uric acid.
[0016] The precursor FeCO3 is calcined at a high temperature, the calcination temperature is 400-600°C, and the time is 1-3 hours to obtain iron oxide (iron oxide particles);
[0017] At least one of the above steps 3) and 4) is performed;
[0018] 5) Preparation of composite carbon nanotube functional filtration membrane:
[0019] Adding pure water to the composite liquid obtained in step 2) to dilute it, the weight ratio of the composite liquid to pure water = 1:4-6, to obtain a diluted solution;
[0020] Then, the rigid intercalation material obtained in step 3) or step 4) is mixed evenly with the diluent, and then sprayed evenly on the surface of the membrane obtained in step 1) by spraying;
[0021] The usage ratio of the rigid intercalation material: diluent = 0.005-0.01 g / 30 ml.
[0022] Note: The purpose of dilution is to form a flowing state, which is convenient for subsequent spraying.
[0023] As an improvement of the preparation method of a composite carbon nanotube functional filtration membrane of the present invention, step 1):
[0024] The PTFE microporous membrane and PET nonwoven material are transported to the same hot pressing roller through two independent conveying rollers at a temperature of 150-290°C and a pressure of 1.5-6 kg / cm 2 The composite membrane is prepared by hot pressing under pressure of 1000 μm (the composite membrane is a hydrophilic PTFE filter membrane).
[0025] As a further improvement of the preparation method of a composite carbon nanotube functional filtration membrane of the present invention, step 2):
[0026] The surfactant is Triton X-100 or sodium dodecylbenzene sulfonate; the adhesive is water-based polyurethane or water-based epoxy resin.
[0027] As a further improvement of the preparation method of a composite carbon nanotube functional filtration membrane of the present invention, step 2): the activation method includes plasma treatment, heat treatment, hydrogen peroxide or acid treatment.
[0028] For example, the heat treatment is as follows: the carbon nanotube powder is activated by calcining at 400±20° C. for 120±20 min to obtain activated carbon nanotube powder.
[0029] As a further improvement of the method for preparing a composite carbon nanotube functional filtration membrane of the present invention, the step 3):
[0030] Add 100±10 ml of pure water to 10 ml of titanium tetrachloride, then add 0.5 g of agar, hydrolyze at 90-100° C. for 90±10 min, then centrifuge (6000-10000 rpm for 10-40 min) to separate the precipitate, and wash the precipitate with pure water;
[0031] The washed precipitate is first dried (at 80-110°C for 20-40 minutes to obtain an off-white powder), and then calcined at 300-600°C for 50-70 minutes (preferably at 400°C for 60 minutes) to obtain titanium dioxide (titanium dioxide particles with a particle size of about 40-60 nm).
[0032] Note: The presence of agar can effectively prevent particles from agglomerating and improve the stability of the solution; washing the precipitate with pure water is to obtain a purer precipitate.
[0033] As a further improvement of the preparation method of a composite carbon nanotube functional filter membrane of the present invention, the step 4): add 0.0012 mol of ferric chloride hexahydrate to 15±1 ml of water, stir evenly (stir until it presents a uniform red color), add 0.6M, 6±1 ml of sodium carbonate solution again and stir (stirring time is 10±2 min), then add 6±1 ml of propylene glycol and 0.4-0.5 g (preferably 0.42 g) of ascorbic acid and stir evenly (stir until it presents a uniform black color); then react at 180±10°C for 16±1 h, then centrifuge (centrifuge at 8000-10000 rpm for 35-45 min), wash the precipitate with water to obtain a precursor FeCO3; then calcine the precursor FeCO3 at 500±50°C for 2±0.2 h to obtain iron oxide.
[0034] Description: Sodium carbonate is mainly used as a mineralizer and pH regulator in the process of preparing iron oxide by the ferric chloride hydrothermal method, affecting the chemical balance and physical conditions of the reaction system. Among them, the mineralizer can increase the solubility of the solute in the hydrothermal solution and change the coefficient of its solubility change with temperature; as a pH buffer, it can adjust the pH of the reaction system and promote the hydrolysis and precipitation of the iron source, thus having an important influence on the formation process of iron oxide and the properties of the final product.
[0035] That is, the present invention uses an appropriate amount of sodium carbonate to perform a preliminary adjustment on the pH value of the solution and can effectively prevent the agglomeration of the product, and then uses ascorbic acid or uric acid as a reducing agent to reduce the solution.
[0036] As a further improvement of the method for preparing a composite carbon nanotube functional filtration membrane of the present invention, the step 5):
[0037] When the rigid intercalation material and the diluent are uniformly mixed, a magnetic stirrer at 200 to 600 rpm is used for a stirring time of 4 to 10 hours;
[0038] During spraying, the spraying distance is set at 8-20 cm, and the spraying time for each time is set at 3-8 s (i.e., the amount of spraying liquid corresponding to each square centimeter is about 0.13-0.15 ml). After each spraying, it is dried at 45-70°C for 5-10 minutes (i.e., after spraying and drying, the next spraying and drying are carried out); the number of spraying is 2-3 times.
[0039] The present invention selects rigid nanomaterials of different structures as intercalation materials, studies the supporting and modifying effects of the microstructure of the intercalation materials on the pore structure of the carbon nanotube membrane, analyzes the influence of the surface chemical properties of the intercalation materials on the physical and chemical properties of the membrane surface and the internal network channel surface, and finally establishes a composite carbon nanotube functional filtration membrane with high wastewater treatment capacity. Compared with the existing preparation process of carbon nanotube composite membranes, this method is more efficient and convenient, and its production equipment and experimental environment have higher tolerance. The present invention realizes the preparation of functional composite membranes by controlling the preparation of carbon nanotube composite liquid, the realization of spraying technology and the construction of intercalation materials, and the obtained composite membrane can reflect high application value in the field of membrane filtration.
[0040] The present invention is based on membrane separation technology and focuses on preparing a composite carbon nanotube functional filtration membrane with a layered assembly structure to achieve effective filtration of sewage, and improves the microstructure of the carbon nanotube membrane by constructing a rigid intercalation material to improve the performance of the composite membrane.
[0041] The outstanding advantage of the present invention is that the carbon nanotube composite membrane preparation technology gives the composite membrane a series of excellent properties. First, through the measurement of the contact angle, because its value is less than 30°, it is shown that the composite membrane has excellent hydrophilicity, which is particularly important in the field of sewage treatment. During the filtration process, it can effectively intercept the dye molecules and oil molecules in the sewage, thereby significantly improving the filtration efficiency and the purity of the water quality. In addition, the efficient separation ability of the carbon nanotube composite membrane enables the sewage to meet the water quality standard requirements after filtration through the membrane, solves the problem of sustainable utilization of water resources, and achieves the purpose of protecting the environment. At the same time, the design of the composite membrane also takes into account the convenience and economy of practical application. Its composite process is simple and efficient, and the membrane has a self-supporting effect by adding a rigid intercalation layer, which avoids the possibility of collapse due to the influence of pressure during repeated use. During the experiment, the membrane was always under a pressure of -0.1MPa, and the membrane did not change significantly after the experiment, indicating that the membrane has excellent stability, reduces the replacement frequency and maintenance cost, and has a wide range of market application prospects.
[0042] The traditional in-situ polymerization method for preparing carbon nanotube membranes is complicated and usually involves multiple steps, including the preparation of catalysts, the introduction of carbon sources, high-temperature treatment, etc., and the chemicals used are often toxic, posing potential risks to the environment and the health of operators. However, the present invention can prepare composite carbon nanotube functional filtration membranes in one step by adopting a spraying method, which not only simplifies the manufacturing process but also avoids the use of toxic chemicals. In general, the present invention achieves simple and effective preparation by optimizing material selection and manufacturing processes, which not only reduces production costs but also improves production efficiency. The flexibility of this process enables rapid response to market demand and meets application scenarios of different scales, whether it is small-batch customization or large-scale production. In addition, its efficient separation capacity not only improves the reuse value of water resources, but also makes a positive contribution to environmental protection.
[0043] At the same time, compared with the current preparation process of carbon nanotube films, the method mentioned in the present invention is more convenient and efficient, can meet the needs of small or large batch production in a short period of time, and has obvious advantages in production efficiency, cost control and environmental friendliness, showing great potential and value in practical applications.
[0044] The invention of the present invention mainly lies in selecting rigid nanomaterials of different structures as intercalation materials, and using a spraying method to prepare a composite carbon nanotube functional filter membrane, which is efficient and convenient. Among them, the intercalation materials are selected from titanium dioxide and iron oxide, and the optimal preparation parameters are determined after multiple experiments, which overcomes the shortcomings of titanium dioxide on the market that is easy to agglomerate and iron oxide has too many impurities. Moreover, the optimal parameter range is set in the preparation process of the intercalation material and the preparation process of the composite carbon nanotube functional filter membrane to increase the quality of the product.
[0045] In summary, the present invention aims at the drawbacks of the complex synthesis method of carbon nanotube membrane and the strict requirements on equipment, and prepares a composite carbon nanotube functional filtration membrane by spraying method. The invention proves that the membrane preparation method is simple and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.
[0047] Figure 1 This is a photograph of the PTFE membrane in the embodiment of the present invention.
[0048] Figure 2 This is a photo of the composite carbon nanotube functional filtration membrane in an embodiment of the present invention.
[0049] Figure 3 This is a photo of a composite carbon nanotube functional filtration membrane with titanium dioxide as an intercalation material in an embodiment of the present invention.
[0050] Figure 4 This is a photo of a composite carbon nanotube functional filtration membrane with iron oxide as an intercalation material in an embodiment of the present invention.
[0051] Figure 5 This is a SEM photo of the composite carbon nanotube functional filtration membrane in an embodiment of the present invention.
[0052] Figure 6 : is a SEM photo of titanium dioxide in an embodiment of the present invention.
[0053] Figure 7 : is a SEM photo of iron oxide in an embodiment of the present invention.
[0054] Figure 8 This is the ultraviolet absorption spectrum of Application Example I of the present invention, in which the samples from left to right are respectively methylene blue solution, filtrate of Application Example a membrane, filtrate of Application Example b membrane, filtrate of Application Example c membrane and water.
[0055] Fig. 9 This is the ultraviolet absorption spectrum of Application Example II of the present invention. The samples in the figure are neutral red solution, filtrate of membrane of Application Example a, filtrate of membrane of Application Example b, filtrate of membrane of Application Example c and water from left to right.
[0056] Fig.10 This is the ultraviolet absorption spectrum of Application Example III of the present invention. The samples in the figure are oil-water emulsion, filtrate of membrane of Application Example a, filtrate of membrane of Application Example b, filtrate of membrane of Application Example c and water from left to right. DETAILED DESCRIPTION
[0057] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0058] The components used in the invention process and subsequent experimental processes of the present invention can be obtained from conventional commercial sources, for example:
[0059] PTFE microporous membrane (0.45 μm), MyBio Biomembrane Technology Co., Ltd.;
[0060] 8% water-based polyurethane solution, Shenzhen Jitian Chemical Co., Ltd.
[0061] PET nonwoven fabric, Changzhou Yinghan Nonwoven Fabric Co., Ltd.;
[0062] Carbon nanotubes, a product of Suzhou Tanfeng Graphene Technology Co., Ltd.;
[0063] Titanium tetrachloride, a product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.;
[0064] Agar, a product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.;
[0065] Ferric chloride hexahydrate, a product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.
[0066] Sodium carbonate, a product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.;
[0067] Ascorbic acid, product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.;
[0068] Glycerol, product of Hangzhou Mi Ke Chemical Instrument Co., Ltd.;
[0069] Methylene blue dye (MB), neutral red dye (NR), products of Sinopharm Chemical Reagent Co., Ltd.;
[0070] Golden Dragon Fish Soybean Oil, a product of Shanghai Kerry Food Industry Co., Ltd.;
[0071] Sodium dodecyl sulfate (SDS), a product of Tianjin Zhiyuan Chemical Reagent Co., Ltd.;
[0072] The pure water used in the experiment was Wahaha purified water.
[0073] Experimental instruments: circulating water ring multi-purpose vacuum pump, product of Shanghai Lichen Instrument Technology Co., Ltd.; magnetic heating stirrer, product of Shanghai Lichen Instrument Technology Co., Ltd.; FA224 electronic balance, product of Shanghai Sunny Hengping Scientific Instrument Co., Ltd.; dead-end filter device, product of Hangzhou Mick Chemical Instrument Co., Ltd.; Cary 60UV-Vis, product of Agilent Technology Co., Ltd.; field emission scanning electron microscope, product of British Zeiss; electric airbrush gun, Guangdong Xiangkong Technology Co., Ltd.; JY-PHb contact angle meter, product of Shanghai Bingjing Instrument Equipment Co., Ltd.; electric constant temperature blast drying oven, product of Shanghai Senxin Experimental Instrument Co., Ltd.; muffle furnace (KSL-1100X), product of Hefei Kejing Material Technology Co., Ltd.; centrifuge (TGL-20B-C), product of Shanghai Anting Scientific Instrument Factory; film laminating machine (TH-PUR, Wuxi Xianhe Automation Equipment Co., Ltd.).
[0074] Embodiment 1,
[0075] (1) Preparation of hydrophilic PFFE membrane
[0076] The PTFE microporous membrane (pore size 0.45 μm) and the PET nonwoven material are transported to the same hot pressing roller through two independent conveyor rollers. 2 The composite membrane is prepared by hot pressing under a pressure of , wherein the composite membrane is a hydrophilic PTFE filter membrane. The composite membrane is made into a roll by a winding machine for standby use.
[0077] The thickness of the PTFE microporous membrane is 0.0015 mm, and the thickness of the nonwoven material is 0.1710 mm.
[0078] (2) Preparation of carbon nanotube composite liquid
[0079] The mass ratio of carbon nanotube powder to TritonX-100 surfactant was set to 1:1;
[0080] Firstly, the carbon nanotube powder is placed in a muffle furnace and calcined at 400° C. for 120 min for activation to obtain activated carbon nanotube powder;
[0081] Then, TritonX-100 surfactant was added to the activated carbon nanotube powder, and the mixture was fully stirred with a glass rod and then placed in a numerically controlled ultrasonic cleaner for 45 minutes to obtain a carbon nanotube / surfactant mixed solution;
[0082] Subsequently, an aqueous polyurethane solution with a mass concentration of 8% was mixed with a mixture of carbon nanotubes / surfactant in a volume ratio of 2:3, and then mechanically stirred at 800 rpm on a magnetic stirrer for 15 minutes, ultrasonically vibrated for 30 minutes, and the "mechanical stirring-ultrasonic vibration" step was repeated twice to finally obtain a uniformly dispersed carbon nanotube composite liquid.
[0083] (3) Preparation of intercalation material titanium dioxide
[0084] 10 ml of titanium tetrachloride and 100 ml of pure water were added to a three-necked flask, followed by 0.5 g of agar, and the titanium tetrachloride was hydrolyzed at 100°C for 90 minutes in the presence of the additive agar. The presence of agar can effectively prevent the aggregation of particles and improve the stability of the solution. Subsequently, a centrifuge was used to separate the precipitate at a speed of 8000 rpm for 20 minutes, and the precipitate was washed 2 to 3 times with pure water (in order to obtain a relatively pure precipitate).
[0085] Then, the washed titanium dioxide powder was dried in an oven at 100° C. for 30 minutes to obtain an off-white powder, and then calcined in a muffle furnace at 400° C. for 60 minutes to obtain titanium dioxide particles (particle size of about 40-60 nm).
[0086] (4) Preparation of intercalation material iron oxide
[0087] Add 0.0012mol of ferric chloride hexahydrate to 15ml of water, stir until a uniform red color appears, then add 0.6M, 6ml of sodium carbonate solution and stir for 10min, then add 6ml of propylene glycol and 0.42g of ascorbic acid and stir until a uniform black color appears. Then place it in a reactor and react at 180°C for 16h, then centrifuge it in a centrifuge at 10000rpm for 40min, wash the precipitate three times with water to obtain the precursor FeCO3, then place the precursor in a muffle furnace and calcine it at 500°C for 2h to obtain the target product iron oxide particles.
[0088] (5) Preparation of composite carbon nanotube functional filtration membrane
[0089] There are three options:
[0090] a) Preparation of carbon nanotube composite filtration membrane
[0091] Take 5 ml of the carbon nanotube composite liquid obtained in step (2), add pure water to make up to 30 ml, use a magnetic stirrer to stir at a speed of 400 rpm for 8 hours under normal temperature and pressure conditions, place it in a spray pot and use an electric spray gun to spray it evenly for 5 seconds at a distance of 15 cm from the PTFE membrane side of the "hydrophilic PTFE filter membrane" obtained in step (1), that is, the amount of spray liquid corresponding to each square centimeter is about 0.14 ml, and then use an oven to dry it at 50°C for 10 minutes, and repeat the "spraying---drying" step twice. The result is named a composite carbon nanotube functional filter membrane.
[0092] b) Preparation of composite carbon nanotube functional filtration membrane with titanium dioxide as intercalation material
[0093] Take 5 ml of the carbon nanotube composite liquid obtained in step (2), add pure water to make up to 30 ml, add 0.01 g of titanium dioxide obtained in step (3), and stir at 400 rpm for 8 hours using a magnetic stirrer under normal temperature and pressure conditions; the subsequent spraying steps are the same as those in scheme a, and the result is named titanium dioxide composite carbon nanotube functional filtration membrane.
[0094] c) Preparation of composite carbon nanotube functional filtration membrane with iron oxide as intercalation material
[0095] Take 5 ml of the carbon nanotube composite liquid obtained in step (2), add pure water to make the volume 30 ml, add 0.005 g of iron oxide obtained in step (4), use a magnetic stirrer to stir at 400 RPM for 8 hours under normal temperature and pressure conditions, and the subsequent spraying steps are the same as those in scheme a. The result is named iron oxide composite carbon nanotube functional filtration membrane.
[0096] Experiment 1
[0097] The experimental method is: use a circulating water ring multi-purpose vacuum pump and a dead-end filter device to filter the solution to calculate the flux. During the experiment, the vacuum pump pressure is controlled at -0.1MPa, the power is turned on, and when the liquid volume of the solution passing through the filter membrane is stable, the liquid volume passing through the membrane per unit time is calculated to obtain the flux.
[0098] Flux formula
[0099]
[0100] Where: J - the flux of solution through the membrane (Lm -2 h -1 ); V is the volume of the solution that passes through the membrane per unit time (L); A is the effective area of the solution that passes through the membrane (m 2 );t——time for solution to pass through the membrane (h).
[0101] Table 1. Relevant performance indicators of composite carbon nanotube functional filtration membrane
[0102]
[0103] It can be seen from Table 1 that the flux of the titanium dioxide composite carbon nanotube functional filtration membrane is larger and the water contact angle is smaller. When the contact angle is less than 90 degrees, the surface is considered to be hydrophilic, and the smaller the angle, the better the hydrophilicity. It can be seen that the titanium dioxide composite carbon nanotube functional filtration membrane is a preferred case.
[0104] Application Example I: Filtration of Methylene Blue Solution
[0105] 5 mg of methylene blue dye powder was added to 1 L of pure water, and stirred at 1200 RPM for 8 h using a magnetic stirrer at room temperature and pressure to obtain a uniform methylene blue dispersion solution. The solution was then filtered using a dead-end filtration device, i.e., the solution was filtered using three composite membranes at a pressure of -0.1 MPa. During the filtration process, the sprayed surface was facing upward, i.e., the methylene blue dispersion solution was in contact with the sprayed surface. The solution before and after filtration was then subjected to ultraviolet absorption spectroscopy, and the results were as follows: Figure 8 shown.
[0106] The specific flux effect is shown in Table 2 below:
[0107] Table 2. Filtration data of composite carbon nanotube functional filtration membrane for methylene blue solution
[0108]
[0109]
[0110] The experiment shows that the carbon nanotube membranes prepared by the three schemes have significant filtration effects, the filtrate is clear, and there is no obvious difference. However, the flux of the membrane obtained by scheme b is larger, and Figure 8 It can be seen that the UV spectrum of the filtrate in scheme b is closer to water, indicating that scheme b has a better effect.
[0111] Application Example II: Filtration of Neutral Red Solution
[0112] 5 mg of neutral red dye powder was added to 1 L of pure water, and stirred at 1200 RPM for 8 h using a magnetic stirrer at room temperature and pressure to obtain a uniform neutral red dispersion solution. The solution was then filtered using a dead-end filtration device, that is, the solution was filtered using three composite membranes at a pressure of -0.1 MPa. During the filtration process, the sprayed surface was facing upward, and the solution before and after filtration was measured by ultraviolet absorption spectrum. The results are shown in the figure. Fig. 9 shown.
[0113] The specific flux effect is shown in Table 3 below:
[0114] Table 3. Filtration data of neutral red solution by composite carbon nanotube functional filtration membrane
[0115]
[0116] The experiment shows that the carbon nanotube membranes prepared by the three schemes have significant filtration effects, the filtrate is clear, and there is no obvious difference. However, the flux of the membrane obtained by scheme b is larger, and Fig. 9 It can be seen that the UV spectrum of the filtrate in scheme b is closer to water, indicating that scheme b has a better effect.
[0117] Application Example III: Filtration of Oil-Water Emulsion
[0118] Add 1 ml of soybean oil and 30 mg of surfactant SDS to 99 ml of pure water, and stir at 1200 RPM for 12 hours using a magnetic stirrer at room temperature and pressure to obtain a uniform oil-water emulsion. Then, use a dead-end filtration device to filter the solution, that is, use three composite membranes to filter the solution at a pressure of -0.1 MPa. During the filtration process, the sprayed surface is facing upward, and the solution before and after filtration is measured by ultraviolet absorption spectrum. The results are as follows: Fig.10 shown.
[0119] The specific flux effect is shown in Table 4 below:
[0120] Table 4. Filtration data of composite carbon nanotube functional filtration membrane for oil-water emulsion
[0121]
[0122]
[0123] The experiment shows that the carbon nanotube membranes prepared by the three schemes have significant filtration effects, the filtrate is clear, and there is no obvious difference. However, the flux of the membrane obtained by scheme b is larger, and Fig.10 It can be seen that the UV spectrum of the filtrate in scheme b is closer to water, indicating that scheme b has the best effect.
[0124] Comparative Example 1: The preparation of intercalation material titanium dioxide in step 3) is cancelled, and the titanium dioxide in scheme b) of step 5) is directly replaced with commercially available titanium dioxide (purity ≥ 99.8%, particle size 60 nm, rutile type) and the rest is the same as scheme b) of step 5).
[0125] The obtained membrane was prepared according to Application Examples I to III. After measurement, the membrane prepared in Comparative Example 1 had a water contact angle of 34.3° and a pure water flux of 42.1421 Lm -2 h -1 , the results are as follows:
[0126] Table 5. Filtration performance of composite carbon nanotube functional filtration membrane in Comparative Example 1
[0127] Filtration of methylene blue solution Filtration of Neutral Red Solution Filtration of oil-water emulsions <![CDATA[Flux (Lm -2 h -1 )]]> 22.4237 29.8584 15.582 Filter Effect The filtrate is light blue The filtrate is light red The filtrate is slightly milky white
[0128] Experiments have shown that although the composite carbon nanotube functional filtration membrane prepared using purchased titanium dioxide has good hydrophilicity, its filtration effect and flux are significantly inferior to those of solution B in the filtration experiments of methylene blue solution, neutral red solution and oil-water emulsion.
[0129] Comparative Example 2: The preparation of intercalation material iron oxide in step 4) is cancelled, and the "iron oxide" in step 5) scheme c) is directly replaced with commercially available "iron oxide (purity ≥ 99%, product specification 300 mesh)", and the rest is the same as step 5) scheme c).
[0130] The obtained membrane was operated according to Application Examples I to III. After measurement, the membrane prepared in Comparative Example 2 had a water contact angle of 35.2° and a pure water flux of 33.4465 Lm -2 h -1 The obtained results are compared with the iron oxide composite carbon nanotube functional filtration membrane (Scheme c) of the present invention as follows:
[0131] Table 6 Filtration performance of composite carbon nanotube functional filtration membrane in comparative example
[0132] Filtration of methylene blue solution Filtration of Neutral Red Solution Filtration of oil-water emulsions <![CDATA[Flux (Lm -2 h -1 )]]> 18.5953 21.1223 9.2339 Filter Effect The filtrate is light blue The filtrate is light red The filtrate is slightly milky white
[0133] Experiments have shown that although the composite carbon nanotube functional filtration membrane prepared using purchased iron oxide has good hydrophilicity, in the filtration experiments of methylene blue solution, neutral red solution and oil-water emulsion, the filtration effect and flux are obviously inferior to those of scheme C. This shows that the iron oxide prepared in the laboratory has better performance.
[0134] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for preparing a composite carbon nanotube functional filtration membrane, characterized in that The steps include: 1) Preparation of organic membrane support: The PTFE microporous membrane and the PET nonwoven material are hot pressed to prepare a composite membrane; 2) Preparation of carbon nanotube composite liquid: After the carbon nanotube powder is activated, a surfactant is added and mixed evenly to obtain a carbon nanotube / surfactant mixed solution; a binder is added to the carbon nanotube / surfactant mixed solution and mixed evenly to obtain a carbon nanotube composite liquid; the mass ratio of the carbon nanotube to the surfactant is 1:1-2, and the volume ratio of the binder to the carbon nanotube / surfactant mixed solution is 2:3-4; 3) Preparation of titanium dioxide as a rigid intercalation material: The titanium tetrachloride is hydrolyzed and centrifuged to obtain a precipitate, which is then washed with water and then dried and calcined to obtain titanium dioxide; 4) Preparation of iron oxide as a rigid intercalation material: The ferric chloride is placed in a reaction kettle and subjected to a hydrothermal reaction under the action of a reducing agent. The temperature of the hydrothermal reaction is in the range of 140 to 240° C. and the time is 10 to 18 hours. After the reaction is completed, the precipitate obtained by centrifugation is washed with water to obtain a precursor FeCO3. The reducing agent is ascorbic acid or uric acid. The precursor FeCO3 is calcined at a high temperature of 400 to 600°C for 1 to 3 hours to obtain iron oxide; At least one of the above steps 3) and 4) is performed; 5) Preparation of composite carbon nanotube functional filtration membrane: Adding pure water to the composite liquid obtained in step 2) to dilute it, the weight ratio of the composite liquid to pure water = 1:4-6, to obtain a diluted solution; Then, the rigid intercalation material obtained in step 3) or step 4) is mixed evenly with the diluent, and then sprayed evenly on the surface of the membrane obtained in step 1) by spraying; The usage ratio of the rigid intercalation material: diluent = 0.005-0.01 g / 30 ml.
2. The method for preparing a composite carbon nanotube functional filtration membrane according to claim 1, characterized in that Step 1): The PTFE microporous membrane and PET nonwoven material are transported to the same hot pressing roller through two independent conveying rollers at a temperature of 150-290°C and a pressure of 1.5-6 kg / cm 2 The composite membrane was prepared by hot pressing under pressure.
3. The method for preparing a composite carbon nanotube functional filtration membrane according to claim 2, characterized in that Step 2): The surfactant is Triton X-100 or sodium dodecylbenzene sulfonate; the adhesive is water-based polyurethane or water-based epoxy resin.
4. The method for preparing a composite carbon nanotube functional filtration membrane according to claim 3, characterized in that The activation method of step 2) includes plasma treatment, heat treatment, hydrogen peroxide or acid treatment.
5. The method for preparing a composite carbon nanotube functional filtration membrane according to any one of claims 1 to 4, characterized in that Step 3): Add 100±10ml of pure water to 10ml of titanium tetrachloride, then add 0.5g of agar, hydrolyze at 90-100℃ for 90±10min, then centrifuge to separate the precipitate, and wash the precipitate with pure water; The washed precipitate is first dried, and then calcined at 300-600° C. for 50-70 minutes to obtain titanium dioxide.
6. The method for preparing a composite carbon nanotube functional filtration membrane according to any one of claims 1 to 5, characterized in that The step 4): add 0.0012 mol of ferric chloride hexahydrate to 15±1 ml of water, stir evenly, then add 0.6 M, 6±1 ml of sodium carbonate solution and stir again, then add 6±1 ml of propylene glycol and 0.4-0.5 g of ascorbic acid and stir evenly; then react at 180±10° C. for 16±1 h, centrifuge again, wash the precipitate with water to obtain a precursor FeCO3; then calcine the precursor FeCO3 at 500±50° C. for 2±0.2 h to obtain iron oxide.
7. The method for preparing a composite carbon nanotube functional filtration membrane according to any one of claims 1 to 6, characterized in that Step 5): When the rigid intercalation material and the diluent are uniformly mixed, a magnetic stirrer at 200 to 600 rpm is used for a stirring time of 4 to 10 hours; During spraying, the spraying distance is set at 8-20 cm, the spraying time for each time is set at 3-8 s, and after each spraying, it is dried at 45-70° C. for 5-10 min; the number of spraying times is 2-3 times.
Citation Information
Patent Citations
Preparation method for super-hydrophilic carbon nanotube nano-porous membrane
CN110038450A
Preparation method and application of MIL-100 (Fe) intercalation g-C3N4 composite film
CN115999368A
Method for manufacturing graphene-carbon nanotube complex structure for water treatment and method for manufacturing membrane using same