Preparation method and application of high-concentration salt lake brine

By using polyphenylene ether and pyridine groups in the salt lake brine, the problem of low lithium ion concentration in the lithium extraction in the salt lake is solved, and efficient purification of high-purity lithium salt solution is achieved, which promotes the raw materials of lithium batteries High purity and low cost production.

CN119056276APending Publication Date: 2024-12-03ZHEJIANG QUZHOU YOUNGDREAM LI-ION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411325647.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing salt lake lithium extraction technology has a problem of low concentration when treating brine with high lithium content, which limits the extraction efficiency and industrial development of high-purity lithium salts.

Method used

Use polyphenylene ether as the substrate and pyridine compounds as the side chain groups to prepare a functional anion exchange membrane through bromination reaction and vacuum defoaming, and assemble it with electrode plates and commercial cationic separators to purify the lithium salt through electrodialysis. Increase lithium ion concentration.

Benefits of technology

It has achieved efficient purification of the lithium ion concentration in the salt lake brine, and obtained a high-purity lithium salt solution, supporting the extraction of high-purity lithium salts in subsequent processes, improving the purity and cost-effectiveness of lithium battery raw materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of high-concentration salt lake brine. The method comprises the following specific steps: 1) carrying out bromination reaction on polyphenyl ether and a bromination reagent under the action of an initiator to obtain a brominated polyphenyl ether solution containing impurities; and 2) dissolving the brominated polyphenyl ether solution in an ethanol solution, filtering and airing to obtain crude brominated polyphenyl ether, dissolving the crude brominated polyphenyl ether in chloroform, continuously adding the ethanol solution to precipitate the brominated polyphenyl ether, pouring out supernate, washing with ethanol for several times, collecting a product, and drying to obtain a brominated polyphenyl ether solid. And 3) dissolving a pyridine compound and brominated polyphenyl ether in NMP (N-Methyl Pyrrolidone) for reaction to obtain a pyridine side group brominated polyphenyl ether compound solution. And 4) heating the solution, carrying out vacuum defoaming treatment, coating on a glass plate, and drying to obtain the thin film. The anion exchange membrane prepared by taking polyphenyl ether as a substrate and a pyridine group as a side chain group has the advantages of high purification capacity and recyclability, and can be widely applied to concentration and purification of salt lake brine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium extraction from salt lakes, and provides a method for preparing high-concentration salt lake brine and its application, specifically the preparation of a functional anion exchange membrane and its application in the field of lithium salt purification. Background Art

[0002] According to the public data of the Ministry of Industry and Information Technology, in 2023, my country's lithium-ion battery (hereinafter referred to as "lithium battery") industry will continue to grow. According to the information of enterprises in the lithium battery industry normative announcement and the calculation of the industry association, the total output of lithium batteries in China will exceed 940GWh, a year-on-year increase of 25%, and the total output value of the industry will exceed 1.4 trillion yuan. It is foreseeable that the lithium-ion battery market will become larger and larger. As the main raw materials of lithium-ion batteries, lithium carbonate and lithium hydroxide will have higher and higher requirements for their purity and cost.

[0003] Salt lake refers to a lake with high concentration of salt on the surface or underground. It is mainly distributed in dry areas and is a very important salinization resource. The composition of salt lakes in different regions varies significantly, which directly leads to the poor versatility of salt lake lithium extraction technology, and to a certain extent limits the development of the salt lake lithium extraction industry. Currently, lithium extraction from salt lakes mainly starts with old brine, and lithium carbonate is produced through a series of processes. The current technical processes mainly include precipitation, extraction, adsorption, membrane separation and electrochemical methods. Different lithium concentrations correspond to different extraction processes. The adsorption method is more suitable for brine with lower concentrations. For salt lakes with higher lithium content and better quality, lithium salt products can be obtained after simple treatment after evaporation and sun exposure of the old brine.

[0004] Salt lakes contain a variety of chemical components, including potassium, lithium, magnesium, sodium, calcium, sulfate, chloride, etc. my country's salt lake brine lithium resources account for more than 80% of the country's total lithium resources, mainly distributed in the Qinghai-Tibet Plateau. The Qinghai-Tibet Plateau is vast and has developed a large number of Quaternary salt lakes, mainly distributed in central and northern Tibet and the Qaidam Basin in Qinghai. The basic characteristics of the Qinghai-Tibet Plateau salt lake brine lithium mines: from the Qaidam Basin to Tibet, the lithium content gradually increases, and the magnesium-lithium ratio gradually decreases. Among them, the average lithium content of the salt lake brine in Tibet is 140mg / L, the average lithium content of the salt lake brine in the Qaidam Basin is 98mg / L, and the average magnesium-lithium ratio is 158. In many salt lakes, the concentration of cations is not high, so the development of a new anion exchange membrane to purify a salt solution with a high lithium ion concentration is conducive to the subsequent extraction of high-purity lithium salts.

[0005] The development of new homogeneous anion exchange membranes generally adopts the method of changing the polymer skeleton and introducing different ionic groups to achieve the performance improvement of anion exchange membranes. Different polymer skeletons, such as polyphenylene ether, polyaryletherketone, polyester, polyamide, polyvinyl alcohol, etc., and different ionic groups, such as pyridinium ion groups, quaternary ammonium ion groups, quaternary phosphonium ion groups, imidazolium salt ion groups, etc., have been used in the development of anion exchange membranes. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing high-concentration salt lake brine and its application, which can efficiently purify the concentration of the brine, making it convenient for a series of subsequent processes to obtain electronic grade lithium carbonate from lithium ions in the high-purity salt solution.

[0007] The present invention is synthesized by the following scheme:

[0008] Step 1) polyphenylene ether and a brominating agent are subjected to a bromination reaction under the action of an initiator to obtain a brominated polyphenylene ether solution containing impurities.

[0009] Step 2) After cooling to room temperature, the brominated polyphenylene ether solution after the reaction is completed is dissolved in an ethanol solution, filtered and dried to obtain a crude brominated polyphenylene ether, and then the crude brominated polyphenylene ether is dissolved in chloroform, and then the ethanol solution is continuously added to precipitate the brominated polyphenylene ether, and the supernatant is poured out and washed with ethanol several times, and the product is collected and dried in an oven to finally obtain a brominated polyphenylene ether solid.

[0010] Step 3) dissolving the pyridine compound and the brominated polyphenylene ether in step 2 in NMP for reaction to change the side chain groups, thereby obtaining a pyridine side group brominated polyphenylene ether compound solution.

[0011] Step 4) The solution obtained in step 3) is subjected to heating vacuum degassing treatment, and then coated on a cleaned glass plate, and a thin film is obtained after drying.

[0012] Step 5) Assemble the anion diaphragm obtained in step 4) with the electrode plate and the commercial cation diaphragm, add the lithium salt solution to perform electrodialysis to purify the lithium salt and perform performance testing.

[0013] Preferably, the bromination reagent in step 1) is one of N-bromosuccinimide, 1,3-dibromo-5,5-dimethylhydantoin, pyridinium tribromide, carbon tetrabromide, and 5,5-dibromo-2,2-dimethyl-4,6-diketo-1,3-dioxane.

[0014] Preferably, the initiator in step 1) is one of azobisisobutyronitrile, dimethyl azobisisobutyrate, azobisisoheptanenitrile and azoisobutylcyanamide.

[0015] Preferably, in step 1), the molar ratio of the bromination agent to the initiator to the polyphenylene ether is 3-5:0.01-0.04:1

[0016] Preferably, the reaction temperature in step 1) is 120-150° C., and the reaction time is 2-6 hours.

[0017] Preferably, in step 2), the dissolution ratio of brominated polyphenylene ether to ethanol is 20-30 g / L, the dissolution ratio of brominated polyphenylene ether to chloroform after drying is 2-3 g / L, and the ratio of brominated polyphenylene ether precipitated in ethanol solution is 20-30 g / L.

[0018] Preferably, in step 2), the total amount of ethanol used for washing is 0.1-1 g / L, and the number of washing times is 2-4 times.

[0019] Preferably, the yield of brominated polyphenylene ether in step 2) is 85-90%.

[0020] Preferably, the pyridine compound in step 3) is 4-ethylpyridine, 3-butylpyridine, 2-hydroxymethylpyridine, 2-(tribromomethylsulfonyl)pyridine, 2-amino-4-chloro-6-methylpyridine, or 2-fluoro-5-iodopyridine.

[0021] Preferably, in step 3), the ratio of pyridine compound to brominated polyphenylene ether is 0.8-1.2:1.

[0022] Preferably, in step 3), the solid-liquid ratio is 0.1-0.2:1.

[0023] Preferably, in step 3), the reaction temperature is 10-40° C. and the reaction time is 24-72 h.

[0024] Preferably, the heating temperature for degassing in step 4) is 40-60°C, and the degassing pressure is 10-100Pa.

[0025] Preferably, the coating area in step 4) is generally 100-1000cm 2 The thickness of the obtained film is generally 100-200μm.

[0026] Preferably, the drying temperature in step 4) is 40-60° C. and the drying time is 24-72 hours.

[0027] Preferably, the lithium salt solution described in step 5) simulates salt lake brine and contains one or more of lithium carbonate, lithium hydroxide, sodium hydroxide, sodium chloride, magnesium chloride, sodium sulfate and silicon chloride.

[0028] Preferably, the simulated salt lake brine in step 5) has a lithium content of 100-1500 mg / L, a sodium content of 5-200 mg / L, a magnesium content of 0.01-100 mg / L, and a chlorine content of 50-200 mg / L.

[0029] Preferably, the ion concentration in the high-purity lithium salt solution obtained by the present invention is ≥3 g / L, which can efficiently purify the ion concentration in the brine so that the solution can be screened and utilized later.

[0030] Furthermore, the anion exchange membrane prepared by the present invention can be widely used in the concentration and purification of salt lake brine.

[0031] The beneficial effects of the present invention are as follows:

[0032] The anion exchange membrane prepared by the method of the present invention uses polyphenylene ether as a substrate and pyridine groups as side chain groups. The anion exchange membrane has the advantages of strong purification ability and recyclability, and can be widely used in the purification technology of salt lake brine. DETAILED DESCRIPTION

[0033] The following technical solutions in the embodiments clearly and completely illustrate the specific content of the present invention, but the embodiments of the present invention are not limited thereto and should not be construed as limiting the scope of protection of the present invention. Any improvements and adjustments made by relevant experimenters in this field based on this patent without creative work shall fall within the scope of protection of the present invention.

[0034] In the following examples, unless otherwise specified, "%" used to indicate concentration refers to mass ratio, ":" used to indicate solid ratio refers to mass ratio, and ":" used to indicate liquid volume refers to volume ratio. Experimental methods without specifying specific experimental conditions were carried out according to common methods in research or operating methods recommended by manufacturers.

[0035] Example 1 A method for preparing high-concentration salt lake brine, the details are as follows:

[0036] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 135℃, then add 14.24g of N-bromosuccinimide and 0.88g of azobisisobutyronitrile, and reflux for 3h. Stop heating, cool to room temperature, drop the reaction mixture into 2000mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 2000mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 200mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 60℃ for 48h, and obtain a milky white flocculent product with a yield of 89.5%.

[0037] First, weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve, and after the brominated polyphenylene ether is completely dissolved, weigh 1.0000g of 4-ethylpyridine, immediately add it to the dissolved brominated polyphenylene ether, stir vigorously, and react at room temperature for 72 hours. After the reaction, a brown viscous liquid is obtained, and the obtained solution is heated and vacuum degassed (heating temperature is 60℃, degassed pressure is 10Pa), and then it is spread on a film, and then placed in an oven at 60℃ for drying for 48 hours to obtain a brown-yellow film with a thickness of 120μm.

[0038] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt solution (including lithium hydroxide, sodium hydroxide, sodium chloride, and magnesium chloride) was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0039] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 10:1. According to the ICP test results, the Li ion concentration was ≥3.3 g / L.

[0040] Example 2 A method for preparing high-concentration salt lake brine, the details are as follows:

[0041] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 150℃, then add 18.62g of 1,3-dibromo-5,5-dimethylhydantoin and 0.88g of azobisisobutyronitrile, and reflux for 2h. Stop heating, cool to room temperature, drop the reaction mixture into 1500mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 1500mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 150mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 50℃ for 72h, and obtain a milky white flocculent product with a yield of 86.5%.

[0042] First, weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve, and after the brominated polyphenylene ether is completely dissolved, weigh 1.0000g of 2-hydroxymethyl pyridine, immediately add it to the dissolved brominated polyphenylene ether, stir vigorously, and react at room temperature for 24 hours. After the reaction, a brown viscous liquid is obtained, and the obtained solution is heated and vacuum degassed (heating temperature is 40℃, degassed pressure is 30Pa), and then it is spread on a film, and then placed in an oven at 50℃ for 48 hours to obtain a brown-yellow film, and the thickness is measured to be 120μm.

[0043] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt (including sodium sulfate, lithium carbonate, sodium chloride, and magnesium chloride) solution was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0044] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 10:1. According to the ICP test results, the Li ion concentration was ≥3.1 g / L.

[0045] Example 3 A method for preparing high-concentration salt lake brine, the details are as follows:

[0046] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 150℃, then add 4.24g of N-bromosuccinimide and 0.92g of dimethyl azobisisobutyrate, and reflux for 4h. Stop heating, cool to room temperature, drop the reaction mixture into 1800mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 1800mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 180mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 60℃ for 24h, and obtain a milky white flocculent product with a yield of 87.2%.

[0047] First, weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve, and after the brominated polyphenylene ether is completely dissolved, weigh 1.0000g of 3-butylpyridine, immediately add it to the dissolved brominated polyphenylene ether, stir vigorously, and react at room temperature for 48h. After the reaction, a brown viscous liquid is obtained, and the obtained solution is heated and vacuum degassed (heating temperature is 50℃, degassed pressure is 50Pa), and then spread on the film, and then put it in an oven at 40℃ for 72h to obtain a brown-yellow film, and the thickness is measured to be 140μm.

[0048] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt solution (including lithium hydroxide, sodium sulfate, sodium chloride, and magnesium chloride) was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0049] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 10:1. According to the ICP test results, the Li ion concentration was ≥3.2 g / L.

[0050] Example 4 A method for preparing high-concentration salt lake brine, the details are as follows:

[0051] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 160℃, then add 18.62g of 1,3-dibromo-5,5-dimethylhydantoin and 0.92g of dimethyl azobisisobutyrate, and reflux for 3h. Stop heating, cool to room temperature, drop the reaction mixture into 2000mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 2000mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 200mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 45℃ for 48h, and obtain a milky white flocculent product with a yield of 88.8%.

[0052] First, weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve, and after the brominated polyphenylene ether is completely dissolved, weigh 1.0000g of 3-butylpyridine and immediately add it to the dissolved brominated polyphenylene ether, stir vigorously, and react at room temperature for 72 hours. After the reaction, a brown viscous liquid is obtained, and the obtained solution is heated and vacuum degassed (heating temperature is 45°C, degassed pressure is 60Pa), and then spread on the film, and then put it in an oven at 55°C for drying for 64 hours to obtain a brown-yellow film with a thickness of 180μm.

[0053] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt solution (including lithium hydroxide, lithium carbonate, sodium sulfate, and sodium chloride) was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0054] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 10:1. According to the ICP test results, the Li ion concentration was ≥3.1 g / L.

[0055] Comparative Example 1

[0056] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 135℃, then add 14.24g of N-bromosuccinimide and 0.88g of azobisisobutyronitrile, and reflux for 3h. Stop heating, cool to room temperature, drop the reaction mixture into 2000mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 2000mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 200mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 60℃ for 48h, and obtain a milky white flocculent product with a yield of 89.5%.

[0057] First weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve it, and after the brominated polyphenylene ether is completely dissolved, heat the resulting solution for vacuum degassing (heating temperature is 40°C, degassing pressure is 30Pa), then spread it into a film, and then put it into an oven for drying at 50°C for 48 hours to obtain a brown-yellow film with a measured thickness of 120μm.

[0058] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt solution (including lithium hydroxide, lithium carbonate, sodium sulfate, and sodium chloride) was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0059] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 3:1. According to the ICP test results, the Li ion concentration was ≥2.5 g / L.

[0060] Comparative Example 2

[0061] Weigh 24g of polyphenylene ether and dissolve it in 200mL of chlorobenzene, heat it to 150℃, then add 18.62g of 1,3-dibromo-5,5-dimethylhydantoin and 0.88g of azobisisobutyronitrile, and reflux for 2h. Stop heating, cool to room temperature, drop the reaction mixture into 1500mL of ethanol solution, filter to obtain crude brominated polyphenylene ether, dry it naturally and dissolve it in chloroform. Add 1500mL of ethanol solution continuously to reversely precipitate to obtain brominated polyphenylene ether, let it stand and pour off the supernatant, add 150mL of ethanol solution to wash, then pour off the solution, filter to obtain pure brominated polyphenylene ether, dry it in a vacuum oven at 50℃ for 72h, and obtain a milky white flocculent product with a yield of 86.5%.

[0062] First weigh 1.0000g of brominated polyphenylene ether, add 8mL of nitrogen methyl pyrrolidone (solid-liquid ratio 0.12:1) as a solvent to dissolve it, and after the brominated polyphenylene ether is completely dissolved, heat the resulting solution for vacuum degassing (heating temperature is 40°C, degassing pressure is 30Pa), then spread it into a film, and then put it into an oven for drying at 50°C for 48 hours to obtain a brown-yellow film with a measured thickness of 120μm.

[0063] The obtained film was used as an anion diaphragm, assembled with a plate and a commercial cation diaphragm, and a lithium salt (including sodium sulfate, lithium carbonate, sodium chloride, and magnesium chloride) solution was added to perform an electrodialysis purification of lithium salt performance test, wherein the lithium content in the lithium salt solution was 200 mg / L, the sodium content was 100 mg / L, the magnesium content was 50 mg / L, and the chlorine content was 100 mg / L. The solution in the concentration chamber was taken out to measure its ion concentration.

[0064] The ratio of the ion concentration of the prepared high ion concentration solution to the ion concentration before membrane treatment was 3:1. According to the ICP test results, the Li ion concentration was ≥2.4 g / L.

[0065] Comparative Example 3

[0066] This comparative example provides a method for preparing high-concentration salt lake brine, which is basically the same as Example 1, except that: the thickness of the obtained brown-yellow film is 100 μm, and a solution with high ion concentration is prepared by using the film. The ratio of its ion concentration detected to the ion concentration before membrane treatment is 8:1, and according to the ICP test results, the Li ion concentration is ≥2.4 g / L.

[0067] Comparative Example 4

[0068] This comparative example provides a method for preparing high-concentration salt lake brine, which is basically the same as Example 1, except that: the thickness of the obtained brown-yellow film is 150 μm, and a solution with high ion concentration is prepared by using the film. The ratio of its ion concentration detected to the ion concentration before membrane treatment is 9:1, and the Li ion concentration is ≥3.0 g / L according to the ICP test results.

[0069] Comparative Example 5

[0070] This comparative example provides a method for preparing high-concentration salt lake brine, which is basically the same as Example 1, except that: the thickness of the obtained brown-yellow film is 200 μm, and a solution with high ion concentration is prepared by using the film. The ratio of its ion concentration detection to the ion concentration before membrane treatment is 8:1, and according to the ICP test results, it is concluded that the Li ion concentration is ≥2.8 g / L.

[0071] The performance results are summarized in Table 1 below.

[0072] Table 1

[0073] Concentration ratio Li ion concentration (g / L) Example 1 10:1 ≥3.3 g / L Example 2 10:1 ≥3.1 g / L Example 3 10:1 ≥3.2 g / L Example 4 10:1 ≥3.1 g / L Comparative Example 1 3:1 ≥2.5 g / L Comparative Example 2 3:1 ≥2.4 g / L Comparative Example 3 8:1 ≥2.4 g / L Comparative Example 4 9:1 ≥3.0 g / L Comparative Example 5 8:1 ≥2.8 g / L

[0074] As shown in Table 1, the amount of bromination reagent and initiator in the process of preparing the film will affect the grafting ratio of pyrrolidone, and ultimately affect the concentration performance and Li ion concentration of the film; on the other hand, the thickness of the film also has a great influence on the concentration ratio and the concentration of Li ions in the concentrated solution. Finally, the film prepared under the conditions of Example 1 showed better concentration performance and higher Li ion concentration.

[0075] In summary, compared with the existing methods, the anion exchange membrane prepared by the method of the present invention with polyphenylene ether as the substrate and pyridine group as the side chain group has the advantages of strong purification and concentration ability and recyclability. The anion exchange membrane prepared by the present invention can be widely used in the concentration and purification technology of salt lake brine.

Claims

1. A method for preparing high-concentration salt lake brine, It is characterized in that The specific steps are as follows: Step 1, subjecting polyphenylene ether to a bromination agent under the action of an initiator to undergo a bromination reaction to obtain a brominated polyphenylene ether solution containing impurities; Step 2, after cooling to room temperature, dissolving the brominated polyphenylene ether solution after the reaction is completed in an ethanol solution, filtering and drying to obtain a crude brominated polyphenylene ether, then dissolving the crude brominated polyphenylene ether in chloroform, and continuously adding an ethanol solution to precipitate the brominated polyphenylene ether, pouring out the supernatant and then washing with ethanol for several times, collecting the product and drying it in an oven to finally obtain a brominated polyphenylene ether solid; Step 3, dissolving the pyridine compound and the brominated polyphenylene ether in step 2 in NMP to react so as to change the side chain groups thereof, thereby obtaining a pyridine side group brominated polyphenylene ether compound solution; Step 4, heating and vacuum degassing the pyridine side group brominated polyphenylene ether compound solution, coating it on a cleaned glass plate, and drying it to obtain a film; Step 5: Use the film obtained in step 4 as an anion diaphragm, assemble it with the electrode plate and the commercial cation diaphragm, add lithium salt solution to perform electrodialysis purification of lithium salt and perform performance test.

2. A method for preparing high-concentration salt lake brine as claimed in claim 1, Features The molar ratio of the bromination reagent, initiator and polyphenylene ether in step 1 is (3-5):(0.01-0.04):

1.

3. A method for preparing high-concentration salt lake brine as claimed in claim 1 or 2, Features The bromination reaction temperature in step 1 is 120-150° C., and the reaction time is 2-6 hours.

4. A method for preparing high-concentration salt lake brine as claimed in claim 1 or 2, Features In step 2, the dissolution ratio of the brominated polyphenylene ether to ethanol is 20-30 g / L, the dissolution ratio of the brominated polyphenylene ether to chloroform after drying is 2-3 g / L, and the ratio of the brominated polyphenylene ether precipitated in the ethanol solution is 20-30 g / L.

5. A method for preparing high-concentration salt lake brine as claimed in claim 1, Features The total amount of ethanol washing in step 2 is 0.1-1 g / L, and the number of washing times is 2-4 times.

6. A method for preparing high-concentration salt lake brine as claimed in claim 2, Features The molar ratio of the pyridine compound to the brominated polyphenylene ether in step 3 is 0.8-1.2:

1.

7. A method for preparing high-concentration salt lake brine as claimed in claim 6, Features In step 3, the mass ratio of the pyridine compound and the brominated polyphenylene ether to the solvent NMP is 0.1-0.2:

1.

8. A method for preparing high-concentration salt lake brine as claimed in claim 2, 6 or 7, Features The coating area in step 4 is 100-1000cm 2 The thickness of the obtained film is 100-200 μm.

9. A method for preparing high-concentration salt lake brine as claimed in claim 8, Features The degassing heating temperature in step 4 is 40-60° C., the degassing pressure is 10-100 Pa, the drying temperature is 40-60° C., and the drying time is 24-72 hours.

10. A method for preparing high-concentration salt lake brine as claimed in claim 1, Features Step 5: using a lithium salt solution to simulate salt lake brine, the lithium salt solution includes lithium carbonate, lithium hydroxide, lithium chloride and lithium sulfate, and also includes several of sodium hydroxide, sodium chloride, magnesium chloride and sodium sulfate; The simulated salt lake brine has a lithium content of 100-1500 mg / L, a sodium content of 5-200 mg / L, a magnesium content of 0.01-100 mg / L, and a chlorine content of 50-200 mg / L; The ion concentration in the lithium salt solution is ≥3g / L, which can efficiently purify the ion concentration in the brine so that the solution can be screened and utilized later.