Block adsorbent as well as synthesis method and application thereof

By synthesizing double ligand mixed Al-MOFs bulk adsorbent on activated carbon fibers in situ, the problems of large mass heat transfer resistance and low loading rate of MOFs are solved, and efficient water vapor adsorption and photothermal conversion are achieved, suitable for drought Regional atmospheric water collection technology.

CN119056416APending Publication Date: 2024-12-03JIANGSU JOSEM ENVIRONMENTAL EQUIP MFG CO LTD

Patent Information

Application Number
CN202411239455.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

As adsorbents, existing metal organic frameworks (MOFs) have problems such as large mass transfer heat transfer resistance, low loading rate, poor photo-heat conversion performance and risk of adhesive blockage, which is difficult to meet the needs of atmospheric water collection technology in arid areas.

Method used

The mixed solvent-thermal method is used to synthesize double-ligand mixed Al-MOFs bulk adsorbent on activated carbon fibers in situ. The activated carbon fiber with high photothermal conversion performance isotherm of MOFs by adjusting the ratio of double-ligands. Curve avoids additional adhesive, and achieves close bonding between MOFs and substrate.

Benefits of technology

It improves the loading rate and photothermal conversion efficiency of the adsorbent, reduces the desorption activation energy, enhances the water vapor adsorption capacity under low humidity conditions, and is suitable for water collection systems in different arid areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056416A_ABST
    Figure CN119056416A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of chemical material synthesis and atmospheric water collection, in particular to a block adsorbent and a synthesis method and application thereof. The synthesis method comprises the following steps: dissolving two organic dicarboxylic acids serving as double ligands in an organic solvent, adding deionized water, and uniformly stirring to obtain a double-ligand uniform dispersion liquid; and adding modified activated carbon fibers containing aluminum ions into the double-ligand uniform dispersion liquid, and reacting under a closed condition to obtain the block adsorbent. The prepared block adsorbent is small in mass transfer and heat transfer resistance and good in photothermal conversion efficiency, adhesive particles are tightly combined with the surface of a base material, the loading rate is high, the moisture absorption capacity is improved, the moisture absorption effect can be adjusted through the proportion of double ligands, and the block adsorbent is suitable for water collection systems in different arid regions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical material synthesis and atmospheric water collection, and in particular to a block adsorbent and a synthesis method and application thereof. Background Art

[0002] Water shortage and energy shortage are two major challenges that threaten human life and hinder social and economic development. Although 70% of the earth's surface is ocean, only 0.5% of the world's water resources are used for human life, and the existing freshwater resources such as rivers, lakes and groundwater are being lost due to human pollution and environmental damage, making it difficult to meet the normal water demand in inland or desert areas. The use of traditional fossil energy such as coal, oil and natural gas will aggravate environmental pollution and affect human life and health. At the same time, the depletion of traditional energy is also threatening the development of society. Therefore, the development and utilization of new energy such as energy, hydrogen energy, solar energy, and nuclear energy is particularly important. In this regard, using adsorbent-based solar-driven atmospheric water harvesting technology (SSAWH) to capture moisture in the air is a feasible strategy that is expected to alleviate water shortage pressure in arid areas and improve energy utilization efficiency in the future.

[0003] The performance of the adsorbent largely determines the water collection capacity of atmospheric water harvesting (AWH). Traditional adsorbents such as silica gel, zeolite, hygroscopic salts, etc., either require a large amount of regeneration energy input or need to be in high relative humidity (RH) air to achieve sufficient water absorption capacity, which cannot meet the requirements of AWH technology. In contrast, metal organic frameworks (MOFs) are widely used in AWH technology research in arid areas due to their excellent cyclic stability, high water absorption capacity at low humidity, low regeneration energy, and structural adjustability.

[0004] However, there are some problems with the current use of MOFs as adsorbents. On the one hand, powdered MOFs have large resistance to mass and heat transfer, and MOFs are usually white or light-colored, with weak light absorption and poor photothermal conversion performance, and cannot rely on themselves to obtain enough solar energy to drive water desorption. On the other hand, the adsorption and desorption isotherm of a single metal organic framework (MOF) synthesized using a dicarboxylic acid is fixed, and can only be used in occasions with a certain humidity; for other humidity occasions, only MOFs synthesized with other dicarboxylic acids can be used; for some humidity occasions, suitable MOF materials cannot be found at present, and different MOF particle powders can only be mixed in proportion to achieve this. When they are loaded on the substrate, due to the small interaction between different MOF particles and between MOF particles and the substrate, an external adhesive is usually required, which not only reduces the loading rate of the MOF adsorbent, but also poses the risk of the adhesive clogging the MOF pores. To address the above problems, the current solution is to carrier-based MOFs and combine MOFs with photothermal materials to prepare composite adsorbents. However, the weak interface between the carrier and MOFs will cause the MOFs coating to be unstable and easy to fall off. The introduction of photothermal agents will also reduce the water absorption of the composite adsorbent. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a block adsorbent with small mass and heat transfer resistance and high loading rate, and a synthesis method and application thereof.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for synthesizing a block adsorbent, comprising the following steps: dissolving two organic dicarboxylic acids as dual ligands in an organic solvent, adding deionized water, and stirring to obtain a uniform dispersion of the dual ligands; adding modified activated carbon fibers containing aluminum ions (Al2O3) to the uniform dispersion of the dual ligands; 3+ -MACF), react under closed conditions to obtain a bulk adsorbent.

[0007] Another technical solution adopted by the present invention is: a block adsorbent is prepared by adopting the above-mentioned synthesis method of the block adsorbent.

[0008] Another technical solution adopted by the present invention is: application of the above-mentioned block adsorbent in atmospheric water collection.

[0009] The beneficial effects of the present invention are as follows: the synthesis method of the present invention uses a mixed solvent thermal method to in-situ synthesize an activated carbon fiber-based dual-ligand mixed Al-MOFs bulk adsorbent on activated carbon fiber, and the MOFs powder is evenly dispersed on the surface and gaps of the substrate, which can solve the problem of large resistance to mass transfer and heat transfer. In the synthesis process, activated carbon fiber with high photothermal conversion performance is selected as the substrate, which can effectively enhance the photothermal conversion efficiency of the adsorbent, and eliminate the need for additional photothermal agents, thereby increasing the loading rate of the MOFs adsorbent and thus increasing the moisture absorption capacity; through the in-situ synthesis process, the adsorbent particles can be closely combined with the substrate surface without the need for additional adhesives, which can increase the loading rate of the MOFs adsorbent and increase the heat and mass transfer rate of the adsorbent in the adsorption and desorption process; by selecting dual ligands as adsorbents, the ratio of ligands can be adjusted to adjust the mixed MOFs between the limits of the two parent MOFs, which is suitable for water collection systems in different arid areas. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 Shown are XRD spectra of the adsorbents obtained in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2;

[0011] Figure 2 Shown are SEM images of the adsorbents obtained in Example 1 of the present invention and Comparative Examples 1-2;

[0012] Figure 3 Shown are water vapor adsorption isotherms of the adsorbents obtained in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2;

[0013] Figure 4 Shown are water adsorption kinetic curves of the adsorbents obtained in Example 1 of the present invention and Comparative Example 3;

[0014] Figure 5 Shown are light absorption curves of the activated carbon fiber substrate of the present invention and the adsorbents obtained in Example 1 and Comparative Example 3 in the range of 200 to 2500 nm;

[0015] Figure 6 The graph shown is a graph showing the change of the surface temperature of the adsorbent obtained in Example 1 of the present invention and Comparative Example 3 under simulated sunlight irradiation over time. DETAILED DESCRIPTION

[0016] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.

[0017] A method for synthesizing a bulk adsorbent comprises the following steps: dissolving two organic dicarboxylic acids as dual ligands in an organic solvent, adding deionized water, and stirring to obtain a dual ligand uniform dispersion; adding modified activated carbon fibers containing aluminum ions to the dual ligand uniform dispersion, reacting under closed conditions, and obtaining a bulk adsorbent.

[0018] From the above description, it can be seen that the beneficial effect of the present invention is that the present invention uses a mixed solvent thermal method to in-situ synthesize an activated carbon fiber-based dual-ligand mixed Al-MOFs bulk adsorbent on activated carbon fiber. The synthesis process has the following advantages:

[0019] (1) MOFs powder is loaded. Since the modified activated carbon fiber containing aluminum ions has a high specific surface area, the adsorbent (MOFs powder) is evenly dispersed on the surface and in the gaps of the substrate, which can solve the problem of high mass transfer and heat transfer resistance.

[0020] (2) The adsorbent particles can form a tight coating on the substrate surface through the in-situ synthesis process, without the need for additional adhesives. The loading rate is high, and the adsorbent particles are tightly connected, which can not only solve the problem of easy powder loss of the adsorbent, but also avoid the adsorbent being blocked by the adhesive. What is even more valuable is that due to the in-situ process, the synthesized MOFs adsorbent particles are evenly dispersed, and there is no adhesive that can generate thermal resistance, which makes the heat and mass transfer rate of the adsorbent in the adsorption and desorption process fast, and its desorption activation energy is significantly reduced.

[0021] (3) The use of activated carbon fibers with high photothermal conversion performance as the substrate eliminates the need for the addition of additional photothermal agents, thereby maximizing the loading rate of the MOFs adsorbent and increasing the moisture absorption capacity.

[0022] (4) By using dual ligands and adjusting the ratio of the ligands, the water vapor adsorption isotherm of MOFs can be regulated, so that the hybrid MOFs can be modulated between the limits of the two parent MOFs, which is suitable for water collection systems in different arid areas.

[0023] Furthermore, the organic solvent is N,N-dimethylformamide (DMF).

[0024] Furthermore, the method also includes cleaning and drying steps after the reaction.

[0025] Furthermore, the specific method of cleaning is: cleaning with ethanol and deionized water respectively.

[0026] From the above description, it can be seen that the unreacted aluminum salt and residual DMF can be removed after washing with ethanol and deionized water.

[0027] Furthermore, the preparation method of the modified activated carbon fiber containing aluminum ions comprises the following steps:

[0028] S1: The activated carbon fiber (ACF) is soaked in an oxidant, taken out, washed with deionized water until neutral, and then dried to obtain oxidized activated carbon fiber (OACF);

[0029] S2: Aluminum salt and a water-soluble film-forming agent are added to deionized water to prepare a film-forming mixed solution containing aluminum ions; the film-forming mixed solution is dropped onto the surface of the oxidized activated carbon fiber to completely wet it, and after drying, a modified activated carbon fiber containing aluminum ions is obtained.

[0030] From the above description, it can be seen that in the process of preparing the modified activated carbon fiber containing aluminum ions, the activated carbon fiber is used as the substrate, and the carboxyl, hydroxyl and other oxygen-containing polar groups of the substrate are increased under the oxidation of the oxidant to improve its hydrophilicity; then the substrate is modified with a water-soluble film-forming agent to prepare the modified activated carbon fiber containing aluminum ions. This modification process can enhance the interfacial force between the mixed Al-MOFs and the substrate, and promote the effective loading of the mixed Al-MOFs on the substrate.

[0031] Furthermore, the oxidant includes at least one of concentrated sulfuric acid, concentrated nitric acid, hydrogen peroxide, potassium permanganate and potassium dichromate.

[0032] Preferably, the oxidizing agent is concentrated sulfuric acid.

[0033] From the above description, it can be seen that concentrated sulfuric acid has better oxidation modification effect and corrosiveness on the substrate.

[0034] Further, the activated carbon fibers are immersed in the oxidant for 1.5 to 2.5 hours.

[0035] From the above description, it can be seen that if the immersion time of activated carbon fiber in the oxidant is too short, the oxidation effect is not obvious, and if it is too long, it will affect the production efficiency.

[0036] Furthermore, the water-soluble film-forming agent includes any one of chitosan hydrochloride, carboxymethyl chitosan, sodium alginate, sodium carboxymethyl cellulose and polyvinyl pyrrolidone.

[0037] Preferably, the water-soluble film-forming agent is chitosan hydrochloride.

[0038] From the above description, it can be seen that chitosan hydrochloride has better film-forming effect and hydrophilicity on the substrate, and has a more advantageous price.

[0039] Furthermore, the aluminum salt is any one of aluminum nitrate, aluminum sulfate, aluminum chloride, and aluminum acetate.

[0040] Preferably, the aluminum salt is aluminum nitrate.

[0041] From the above description, it can be seen that the solubility of aluminum nitrate and the loading amount on the substrate are better.

[0042] Furthermore, the biligand is any two of 3,5-pyrazoledicarboxylic acid, fumaric acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid and isophthalic acid.

[0043] Preferably, the biligand is 3,5-pyrazoledicarboxylic acid and fumaric acid.

[0044] From the above description, it can be seen that when the dual ligands are 3,5-pyrazoledicarboxylic acid and fumaric acid, the ligands and Al 3+ The competitive rate is faster and the price of the ligand is lower, and the steep adsorption range of the resulting MOFs water vapor adsorption isotherm is more suitable for arid areas.

[0045] Furthermore, the molar ratio of the two organic dicarboxylic acids in the dual ligand is 8:2 to 2:8.

[0046] Furthermore, the molar ratio of the dual ligand to the aluminum ions in the modified activated carbon fiber containing aluminum ions is 0.6:1 to 1.5:1.

[0047] Preferably, the molar ratio of the two organic dicarboxylic acids in the dual ligand is 7:3 to 3:7; the molar ratio of the dual ligand to the aluminum ion in the modified activated carbon fiber containing aluminum ions is 0.8:1 to 1.2:1.

[0048] From the above description, we can know that by changing the ratio of the two ligands, a series of mixed MOFs can be obtained to adjust the MOFs water vapor adsorption isotherm, so that the mixed MOFs can be adjusted between the limits of the two parent MOFs, which can be applied to water collection systems in different arid areas. If the ratio of a certain ligand is too high, only a single MOF can be obtained; on the contrary, if the ratio of a certain ligand is too low, its synthesis rate is too slow, and the corresponding MOF cannot be obtained.

[0049] Furthermore, the reaction conditions are: reacting at 80-160° C. for 11-13 hours.

[0050] From the above description, it can be seen that if the synthesis temperature is too low, the yield of the mixed MOFs is too low; if the synthesis temperature is too high, the purity of the product is low and its product performance is reduced. If the reaction time is short, the yield of the mixed MOFs obtained is low; if the reaction time is too long, the efficiency of the mixed MOFs obtained is low. Therefore, the reaction conditions are limited to: react at 80-160°C for 11-13h.

[0051] Another technical solution adopted by the present invention is: a block adsorbent is prepared by adopting the above-mentioned synthesis method of the block adsorbent.

[0052] Furthermore, the dual-ligand mixed Al-MOFs in the bulk adsorbent are any two of MOF-303, Al-Fum (A520), MOF-160, MOF-333 and CAU-10-H.

[0053] Preferably, the dual-ligand mixed Al-MOFs are MOF-303 and Al-Fum.

[0054] Another technical solution adopted by the present invention is: application of the above-mentioned block adsorbent in atmospheric water collection.

[0055] Further, the application of the above block adsorbent in atmospheric water collection by solar-driven adsorbent desorption in arid areas

[0056] From the above description, it can be seen that the block adsorbent of the present invention uses activated carbon fiber with high photothermal conversion performance as the substrate, which can effectively enhance the photothermal conversion performance of the adsorbent, thereby realizing solar-driven adsorbent desorption of water and improving energy utilization efficiency. The block adsorbent has lower desorption activation energy, which can effectively reduce the energy consumption of the water collection system, and has a high water vapor adsorption capacity under low humidity conditions (<40% RH).

[0057] The reagents and instruments used in the following examples are conventional products that can be purchased from the market.

[0058] The following Examples 1 to 7 and Comparative Examples 1 to 3 contain Al 3+ Modified activated carbon fiber (Al 3+ -MACF) preparation method, the steps are as follows:

[0059] S1: Immerse the cut activated carbon fiber with a size of 3×3×0.3 cm in concentrated sulfuric acid with a mass fraction of 98.3% for 2 h, take it out and wash it with deionized water until it is neutral, and place it in an oven to dry to obtain oxidized activated carbon fiber.

[0060] S2: 1.14 g (3.0 mmol) Al(NO3)3·9H2O was dissolved in 3 mL 0.025 g / mL chitosan hydrochloride (CTS) solution, and magnetic stirring was performed to form a milky white mixed solution; the mixed solution was evenly dripped onto the surface of the oxidized activated carbon fiber to completely wet it, and then placed in an oven at 60 °C to dry to obtain Al-containing 3+ Modified activated carbon fiber (Al 3+ -MACF).

[0061] Embodiment 1 of the present invention is: a method for preparing an activated carbon fiber-based mixed Al-MOFs block adsorbent containing MOF-303 and Al-Fum, the steps are as follows:

[0062] S1: According to the ratio of 3 mmol of the total amount of the dual ligand and 5 / 5 of the molar ratio of the dual ligand, 0.27 g (1.5 mmol) of 3,5-pyrazoledicarboxylic acid and 0.174 g (1.5 mmol) of fumaric acid were dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a dual ligand dispersion.

[0063] S2: Transfer the dual ligand dispersion to a polytetrafluoroethylene-lined reactor and then add Al 3+ -MACF is immersed in it, and the dual ligand and Al 3+ -Al in MACF 3+ The molar ratio of MOF-303 and Al-Fum is 1:1. After the reactor is sealed, it is placed in a muffle furnace at a crystallization temperature of 110°C for reaction for 12 hours and cooled to room temperature to obtain a substrate loaded with mixed Al-MOFs. The substrate loaded with mixed Al-MOFs is taken out, and washed alternately with ethanol and deionized water for 3 times to remove unreacted aluminum salt and residual DMF, and then placed in a vacuum drying oven at 120°C for 12 hours to obtain activated carbon fiber-based mixed Al-MOFs (mixed Al-MOFs / MACF) containing MOF-303 and Al-Fum.

[0064] Embodiment 2 of the present invention is:

[0065] The only difference between Example 2 and Example 1 is: S1: According to the ratio of the total amount of the dual ligand being 3 mmol and the molar ratio of the dual ligand being 7 / 3, 0.378 g (2.1 mmol) of 3,5-pyrazoledicarboxylic acid and 0.104 g (0.9 mmol) of fumaric acid were respectively dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a dual ligand dispersion.

[0066] Embodiment 3 of the present invention is:

[0067] The only difference between Example 3 and Example 1 is: S1: According to the ratio of the total amount of the dual ligand being 3 mmol and the molar ratio of the dual ligand being 3 / 7, 0.162 g (0.9 mmol) of 3,5-pyrazoledicarboxylic acid and 0.244 g (2.1 mmol) of fumaric acid were respectively dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a dual ligand dispersion.

[0068] Comparative Example 1 of the present invention is: a method for preparing an activated carbon fiber-based MOF-303 block adsorbent, the steps are as follows:

[0069] S1: Under magnetic stirring, 0.54 g (3 mmol) of 3,5-pyrazoledicarboxylic acid was dissolved in 5 mL of DMF to form a DMF solution containing 3,5-pyrazoledicarboxylic acid; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a 3,5-pyrazoledicarboxylic acid dispersion.

[0070] S2: Transfer the 3,5-pyrazoledicarboxylic acid dispersion to a 100 mL polytetrafluoroethylene-lined reactor and then add Al 3+ -MACF is immersed in it, and the ligand and Al 3+ -Al in MACF 3+ The molar ratio of was 1:1, and the reactor was sealed and placed in a muffle furnace at a crystallization temperature of 110°C for reaction for 12 hours, and then cooled to room temperature to obtain a substrate loaded with MOF-303; the substrate loaded with MOF-303 was taken out, and washed alternately with ethanol and deionized water for 3 times to remove unreacted aluminum salt and residual DMF, and then vacuum dried at 120°C to obtain activated carbon fiber-based MOF-303 (MOF-303 / MACF).

[0071] Comparative Example 2 of the present invention is: a method for preparing an activated carbon fiber-based Al-Fum block adsorbent, the steps are as follows:

[0072] S1: Under magnetic stirring, 0.348 g (3 mmol) of fumaric acid was dissolved in 5 mL of DMF to form a DMF solution containing fumaric acid; the DMF solution was added dropwise into 30 mL of deionized water and stirred for 20 min to obtain a fumaric acid dispersion.

[0073] S2: Transfer the fumaric acid dispersion to a 100 mL polytetrafluoroethylene-lined reactor and then add Al 3+ -MACF is immersed in it, and the ligand and Al 3+ -Al in MACF 3+ The molar ratio of is 1:1, the reactor is sealed and placed in a muffle furnace at a crystallization temperature of 110°C for reaction for 12 hours, and then cooled to room temperature to obtain a substrate loaded with Al-Fum; the substrate loaded with Al-Fum is taken out, and washed alternately with ethanol and deionized water for 3 times to remove unreacted aluminum salt and residual DMF, and then vacuum dried at 120°C to obtain activated carbon fiber-based Al-Fum (Al-Fum / MACF).

[0074] Comparative Example 3 of the present invention is: a method for preparing a mixed Al-MOFs powder adsorbent containing MOF-303 and Al-Fum, the steps are as follows:

[0075] S1: According to the ratio of 3 mmol of the total amount of the dual ligand and 5 / 5 of the molar ratio of the dual ligand, 0.27 g (1.5 mmol) of 3,5-pyrazoledicarboxylic acid and 0.174 g (1.5 mmol) of fumaric acid were dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; 1.14 g (3 mmol) of Al(NO3)3·9H2O was dissolved in 30 mL of deionized water, and stirred evenly to form Al 3+ Solution; Add the DMF solution dropwise to the Al 3+ The solution was stirred for 20 min to obtain a double ligand containing 3,5-pyrazoledicarboxylic acid and fumaric acid and Al 3+ of the mixed reaction solution.

[0076] S2: The mixed reaction liquid prepared in S1 was transferred to a polytetrafluoroethylene-lined reactor. The reactor was sealed and placed in a muffle furnace at 110°C for 12 hours, and then cooled to room temperature to obtain a white suspension. After centrifugation, it was washed alternately with DMF and methanol for 3 times, and then placed in a vacuum drying oven at 120°C for 12 hours to obtain a mixed Al-MOFs powder containing MOF-303 and Al-Fum.

[0077] The adsorbents obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested, and the test results are as follows:

[0078] (1) XRD spectra of the adsorbents obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were tested. The test results are shown in Figure 1 .from Figure 1 It can be seen that Examples 1 to 3 use 3,5-pyrazoledicarboxylic acid and fumaric acid in three molar ratios of 5 / 5, 7 / 3, and 3 / 7 as dual ligands, and the characteristic diffraction peaks of the prepared mixed Al-MOFs / MACFs are the same, and their diffraction peaks coincide with the diffraction peaks of MOF-303 in Comparative Example 1 and the diffraction peaks of Al-Fum in Comparative Example 2, and no new peaks appear, proving that the mixed Al-MOFs containing different ratios of MOF-303 and Al-Fum were successfully synthesized in situ on the activated carbon fiber substrate using the mixed solvent thermal method.

[0079] (2) SEM images of the adsorbents obtained from Example 1 and Comparative Examples 1-2. The test results are shown in Figure 2 .from Figure 2 It can be seen that the MOF-303 prepared in Comparative Example 1 is a regular octahedral shape, the Al-Fum crystal prepared in Comparative Example 2 is a regular strip cluster, and the mixed Al-MOFs / MACF obtained in Example 1 is a spherical structure; the difference in their microstructures indicates that 3,5-pyrazoledicarboxylic acid and fumaric acid ligands have a significant effect on the Al 3+ Competition for metal sites leads to the reconstruction of the MOF framework.

[0080] (3) The water vapor adsorption isotherms of the adsorbents obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were tested. The test results are shown in Figure 3 . Figure 3 The results show that the adsorption curves of mixed Al-MOFs / MACFs with different ratios obtained in Examples 1 to 3 can be adjusted between MOF-303 / MACF and Al-Fum / MACF, indicating that the water vapor adsorption curves of mixed Al-MOFs / MACFs can be adjusted by changing the ligand ratio. All samples in Examples 1 to 3 have high water vapor adsorption capacity under low humidity, indicating that the mixed Al-MOFs / MACFs obtained in the present invention can be applied to atmospheric water collection systems in different arid areas by adjusting the ligand ratio.

[0081] (4) The water adsorption kinetic curves of the adsorbents obtained in Example 1 and Comparative Example 3 were tested. The test results are shown in Figure 4 .Depend on Figure 4 The results show that the sample in Example 1 has a faster water adsorption rate than the sample in Comparative Example 3, indicating that the MOFs carrier can increase the heat and mass transfer rates of MOFs in the process of adsorbing water vapor, and can shorten the adsorption cycle in practical applications.

[0082] (5) The light absorption curves of the activated carbon fiber substrate and the adsorbents obtained in Example 1 and Comparative Example 3 in the range of 200 to 2500 nm were tested by UV-vis-NIR spectrometer. The test results are shown in Figure 5 . Figure 5 The results show that the activated carbon fiber substrate and the sample of Example 1 exhibit better light absorption performance than the sample of Comparative Example 3 in the ultraviolet (UV), visible light (VIS) and near infrared (NIR) wavelength ranges.

[0083] (6) The adsorbents obtained in Example 1 and Comparative Example 3 were tested under a simulated sunlight (100 mW / cm 2 ) The surface temperature changes with time under irradiation. The test results are shown in Figure 6 . Figure 6 The results show that the sample in Example 1 has a faster photothermal conversion rate than the sample in Comparative Example 3; after 40 minutes of sunlight irradiation, the temperature of Comparative Example 3 is only 37.3°C, while the temperature of Example 1 can reach 88.3°C, indicating that activated carbon fiber as a substrate can significantly improve the photothermal conversion capacity of the adsorbent, which is conducive to the use of solar energy to achieve efficient desorption of the adsorbent.

[0084] (7) The desorption temperatures of the adsorbents obtained in Example 1 and Comparative Example 3 at different heating rates were tested. The test results are shown in Table 1.

[0085] Table 1

[0086]

[0087] As shown in Table 1, the desorption temperatures of the adsorbents obtained in Example 1 and Comparative Example 3 are both relatively low (about 60°C), much lower than the existing traditional adsorbents silica gel (150°C) and molecular sieves (250°C). At the same heating rate, the peak temperature of Example 1 is lower than that of Comparative Example 3, and Example 1 has a lower desorption activation energy than that of Comparative Example 3, indicating that loading the mixed Al-MOFs on activated carbon fibers can effectively reduce the mass transfer and heat transfer resistance and reduce the desorption energy consumption.

[0088] Embodiment 4 of the present invention is:

[0089] The only difference between Example 4 and Example 1 is: S1: According to the ratio of the total amount of the dual ligand being 2.4 mmol and the molar ratio of the dual ligand being 5 / 5, 0.216 g (1.2 mmol) of 3,5-pyrazoledicarboxylic acid and 0.139 g (1.2 mmol) of fumaric acid were respectively dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a low concentration of the dual ligand dispersion.

[0090] Embodiment 5 of the present invention is:

[0091] The only difference between Example 5 and Example 1 is: S1: According to the ratio of the total amount of the dual ligand being 3.6 mmol and the molar ratio of the dual ligand being 5 / 5, 0.324 g (1.8 mmol) of 3,5-pyrazoledicarboxylic acid and 0.209 g (1.8 mmol) of fumaric acid were respectively dissolved in 5 mL of DMF, and stirred evenly to form a DMF solution containing the dual ligand; the DMF solution was added dropwise into 30 mL of deionized water, and stirring was continued for 20 min to obtain a high-concentration dual ligand dispersion.

[0092] Embodiment 6 of the present invention is:

[0093] The only difference between Example 6 and Example 1 is that the crystallization temperature is 100°C.

[0094] Embodiment 7 of the present invention is:

[0095] The only difference between Example 7 and Example 1 is that the crystallization temperature is 130°C.

[0096] The mass fraction of the mixed Al-MOFs coating in the mixed Al-MOFs / MACF obtained in Examples 1 to 7 was tested. The test results are shown in Table 2.

[0097] Table 2

[0098] Example Mass fraction of mixed Al-MOFs coating (%) Example 1 66 Example 2 65 Example 3 65 Example 4 59 Example 5 66 Example 6 60 Example 7 62

[0099] It can be seen from Table 3 that the mixed Al-MOFs / MACF has a high coating mass fraction, which is beneficial for the adsorbent to adsorb moisture from the air.

[0100] Embodiment 8 of the present invention is:

[0101] The difference between Example 8 and Example 1 is that: 3+ The oxidant in the preparation of -MACF is concentrated nitric acid and hydrogen peroxide in a volume ratio of 1:1, the water-soluble film-forming agent is carboxymethyl chitosan and sodium alginate in a mass ratio of 1:1, and the aluminum salt is aluminum sulfate and aluminum chloride in a mass ratio of 1:1. The double ligand is 2,4-furandicarboxylic acid and isophthalic acid, the molar ratio of the double ligand is 2:8, and the double ligand and Al 3+ The molar ratio of aluminum ions in -MACF is 1.5:1, the crystallization temperature is 160 °C, and the crystallization time is 11 h.

[0102] Embodiment 9 of the present invention is:

[0103] The difference between Example 9 and Example 1 is that: 3+ The oxidant in the preparation of -MACF is potassium permanganate and potassium dichromate in a volume ratio of 1:1, the water-soluble film-forming agent is sodium carboxymethyl cellulose and polyvinyl pyrrolidone in a mass ratio of 1:1, and the aluminum salt is aluminum acetate in a mass ratio of 1:1. The double ligand is 2,5-furandicarboxylic acid and 2,4-furandicarboxylic acid, the molar ratio of the double ligand is 8:2, and the double ligand and Al 3+ The molar ratio of aluminum ions in -MACF is 0.6:1, the crystallization temperature is 80 °C, and the crystallization time is 13 h.

[0104] In summary, the block adsorbent and its synthesis method and application provided by the present invention have the following advantages:

[0105] (1) The activated carbon fiber-based dual-ligand mixed Al-MOFs prepared by the in-situ synthesis method have a high mixed Al-MOFs coating mass fraction, and the MOFs have a strong bonding force with the substrate and are not prone to falling off, which solves the problem of low mass and heat transfer efficiency caused by the agglomeration of powdered MOFs.

[0106] (2) No adhesive is used during the in situ synthesis, which avoids the problem of adhesives clogging the pores of MOFs adsorbents, thereby maximizing the water adsorption capacity of MOFs.

[0107] (3) Compared with MOFs powder, the mixed Al-MOFs prepared in the present invention has lower desorption activation energy, which can effectively reduce the energy consumption of the water collection system.

[0108] (4) The activated carbon fiber substrate used in the present invention has excellent photothermal conversion performance and low cost, and can effectively enhance the photothermal conversion performance of the adsorbent, thereby realizing solar-driven desorption of water by the adsorbent and improving energy utilization efficiency.

[0109] (5) The hybrid Al-MOFs / MACF prepared in the present invention has a high water vapor adsorption capacity under low humidity conditions of <40% RH, and the water vapor adsorption isotherms of the hybrid Al-MOFs prepared with different ligand molar ratios are modulated between the limits of the two parent MOFs, which can be suitable for different applications.

[0110] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for synthesizing a bulk adsorbent, characterized in that: The following steps are involved: Two organic dicarboxylic acids are dissolved as dual ligands in an organic solvent, and then deionized water is added and stirred to obtain a uniform dispersion of the dual ligands; modified activated carbon fibers containing aluminum ions are added to the uniform dispersion of the dual ligands, and the reaction is carried out under closed conditions to obtain a block adsorbent.

2. The method for synthesizing a bulk adsorbent according to claim 1, characterized in that: The method for preparing the modified activated carbon fiber containing aluminum ions comprises the following steps: S1: soaking the activated carbon fiber in an oxidant, taking it out, washing it with deionized water until it is neutral, and then drying it to obtain oxidized activated carbon fiber; S2: Aluminum salt and a water-soluble film-forming agent are added to deionized water to prepare a film-forming mixed solution containing aluminum ions; the film-forming mixed solution is dropped onto the surface of the oxidized activated carbon fiber to completely wet it, and after drying, a modified activated carbon fiber containing aluminum ions is obtained.

3. The method for synthesizing a bulk adsorbent according to claim 2, characterized in that: The oxidant includes at least one of concentrated sulfuric acid, concentrated nitric acid, hydrogen peroxide, potassium permanganate and potassium dichromate.

4. The method for synthesizing a bulk adsorbent according to claim 2, characterized in that: The water-soluble film-forming agent includes any one of chitosan hydrochloride, carboxymethyl chitosan, sodium alginate, sodium carboxymethyl cellulose and polyvinyl pyrrolidone.

5. The method for synthesizing a bulk adsorbent according to claim 2, characterized in that: The aluminum salt is any one of aluminum nitrate, aluminum sulfate, aluminum chloride and aluminum acetate.

6. The method for synthesizing a bulk adsorbent according to claim 1, characterized in that: The biligands are any two of 3,5-pyrazoledicarboxylic acid, fumaric acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid and isophthalic acid.

7. The method for synthesizing a bulk adsorbent according to claim 1, characterized in that: The molar ratio of the dual ligand to the aluminum ions in the modified activated carbon fiber containing aluminum ions is 0.6:1 to 1.5:

1.

8. The method for synthesizing a bulk adsorbent according to claim 1, characterized in that: The reaction conditions are: reacting at 80-160° C. for 11-13 hours.

9. A bulk adsorbent, characterized in that: The bulk adsorbent is prepared by the synthesis method of any one of claims 1 to 8.

10. Use of the block adsorbent as claimed in claim 9 in atmospheric water collection.

Citation Information

Patent Citations

  • Organic foam-based MOF (Metal Organic Framework) block moisture absorbent as well as mixed solvothermal in-situ synthesis method and application thereof

    CN115975369A

  • Active carbon fiber-based MOFs (Metal-Organic Frameworks) block moisture absorbent as well as mixed solvothermal in-situ synthesis method and application thereof

    CN117463292A

  • A process of making an adsorbent body

    WO2023088982A1

Cited By

  • Allochroic silica gel drying agent, preparation method thereof and allochroic silica gel

    CN120285942A