A dual-functional MOF@COF composite material addresses the limitations of existing SPME fibers by providing enhanced selectivity and stability for halogenated pollutants, enabling sensitive detection in environmental and food samples.
Patent Information
- Application Number
- CN202411215677.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Existing SPME fiber coatings lack specific interaction with target pollutants, resulting in limited extraction efficiency, selectivity, and stability, particularly for halogenated persistent organic pollutants like polybrominated diphenyl ethers (PBDEs).
A dual-functional MOF@COF composite material is prepared by solvothermal synthesis and dual-ligand-assisted strategy, forming a core-shell structure with controlled COF shell thickness, providing multiple interaction sites for enhanced enrichment.
The MOF@COF composite fiber exhibits high selectivity and stability, enabling sensitive detection of trace pollutants such as PBDEs in environmental and food samples with improved sensitivity and specificity.
Smart Images

Figure CN119056424A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a dual-functionalized MOF@COF framework composite coated fiber based on a dual-ligand assisted strategy, specifically, using two polymer ligands to functionalize MOF with amino groups, then in-situ growing imine COF on its surface, and then synthesizing a MOF@COF framework composite material for preparing solid phase microextraction fiber, and by pre-functionalizing MOF or COF, different application requirements can also be met. The present invention belongs to both the field of crystalline porous materials and the field of analytical chemistry. Background Art
[0002] Solid Phase Microextraction (SPME) is a new sample pretreatment technology proposed in the early 1990s that integrates sampling, extraction, enrichment, and injection. Compared with traditional extraction techniques, SPME has the characteristics of no solvent, miniaturization, rapidity, portability, and easy operation. It is also easy to analyze volatile pollutants with gas chromatography or gas chromatography-mass spectrometry. It has been widely used to pre-concentrate and extract target analytes from food, environment, spices, and biological samples. Fiber SPME is the most commonly used extraction form. By coating or polymerizing different coating materials on the surface of the fiber carrier, the target is extracted and enriched by headspace or direct immersion. It is easy to use online and saves time. The coating material is a key factor affecting the extraction efficiency of the target. The commonly used commercial SPME fiber coating materials are mainly based on their polarity and characteristics. According to the principle of "like dissolves like", the target is enriched. It has a wide range of applicability, but often lacks specific interaction with the target. Its extraction efficiency, selectivity, and stability are relatively limited. Therefore, the preparation of novel coated fibers with high selectivity and stability is of great significance for the analysis of trace pollutants.
[0003] New crystalline porous materials refer to porous materials formed by organic molecular units connected by coordination bonds, covalent bonds or supramolecular interactions. According to their different bonding methods, they can be divided into metal organic frameworks (MOFs), covalent organic frameworks (COFs), hydrogen bonded organic frameworks (HOFs), supramolecular organic frameworks (SOFs), etc. Due to their designable long-range ordered structures, high surface areas, accessible voids and easily modified pores, crystalline porous materials have shown great development potential in adsorption separation, heterogeneous catalysis and sensing in recent years. Among them, MOF is a porous polymer formed by metal ions or metal oxygen clusters and organic ligands through coordination bonds, and COF is a crystalline porous polymer material connected by covalent bonds. They have become research hotspots in the field of materials because of their large specific surface area, high porosity, and easy structural regulation. At present, they focus on material synthesis, performance and application research. However, in terms of sample pretreatment, these two materials have some inherent defects. For example, MOF materials are unstable in aqueous solution or to heat, and their structure is prone to collapse. COF materials have good stability but no metal nodes, relatively simple functions, and insufficient specific enrichment capabilities, which to some extent limit the extraction application performance.
[0004] In order to improve the performance of single framework materials, people gradually shifted their research focus to the synthesis of composite materials. Compared with single materials, the composite materials of MOF and COF (MOF / COF) have functional integration and synergistic effects, which enable them to introduce new functional sites to form dual / multifunctional composite materials while overcoming their own shortcomings, showing excellent stability and specificity. At present, MOF / COF composite materials have been widely used in the field of membrane separation due to their strong gas separation ability. They have also begun to be used as adsorbents to extract drug residues and pollutants from complex matrices such as the environment or organisms, showing excellent enrichment performance. Polybrominated diphenyl ethers (PBDEs) are a widely used brominated flame retardant that is ubiquitous in the environment and organisms and pollution is on the rise, which has potential hazards to the environment and human health. As a new type of persistent organic pollutant, PBDEs have become a research hotspot in current environmental science, and it is necessary to develop efficient trace analysis technology. At present, researchers have developed coatings or adsorbents based on COF, MOF, and carbon nanotubes for PBDEs enrichment, but there has been no report on the enrichment of PBDEs by MOF / COF composite materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a solid phase microextraction fiber based on a dual-functional MOF@COF composite material. The MOF@COF coated fiber has good specificity and stability, and can be used to enrich halogenated persistent organic pollutants such as polybrominated diphenyl ethers, organochlorine pesticides, and hydroxylated polychlorinated biphenyls, and can be used in conjunction with GC-MS or LC-MS to perform highly sensitive detection of trace pollution in environmental and food samples.
[0006] To achieve the above object, the present invention adopts the following technical solution: A preparation method of a dual-functional MOF@COF composite solid phase microextraction fiber, the specific process of which includes: (1) Preparation of UiO-66-(OH)2 29.7-49.5 mg of 2,5-dihydroxyterephthalic acid and 34.9-93.5 mg of MCl4 (M = Zr, Hf, Th) were added to 5-15 mL of N,N-dimethylformamide for ultrasonic dissolution, and 1.5-4.5 mL of glacial acetic acid was added as a catalyst. The mixed solution was transferred to a 25 mL polytetrafluoroethylene-lined autoclave and reacted at 100-140 °C for 24 h. The obtained product was then washed with ethanol 6 times, centrifuged at 5000-8000 rpm for 5 min, and the precipitate was collected and vacuum dried overnight at 60-80 °C to obtain UiO-66-(OH)2.
[0007] (2) Surface amino functionalization of UiO-66-(OH)2 75-125 mg of UiO-66-(OH)2 was placed in a round-bottom flask containing 25 mL of ethanol and dispersed evenly by ultrasonication. 5 mL of an ethanol mixed solution containing 70-120 mg / mL polyethyleneimine and polyvinylpyrrolidone was slowly added dropwise under stirring. The mixture was magnetically stirred at room temperature for 12-24 h. The solid product was then washed four times with ethanol, centrifuged at 5000-8000 rpm for 5 min, and the precipitate was collected and dried in vacuo at 60-80 °C overnight to obtain amino-functionalized UiO-66-(OH)2.
[0008] (3) Preparation of UiO-66-(OH)2@COF-OCH3 composite materials 5-35 mg of amino-functionalized UiO-66-(OH)2, 1.2-4.6 mg of 2,5-dimethoxyterephthalaldehyde and 1.4-5.6 mg of 1,3,5-tri(4-aminophenyl)benzene were added into a round-bottom flask containing 4-8 mL of a mixed solvent of n-butanol / o-dichlorobenzene (v:v=1:1), dissolved by ultrasound, and then 80-120 μL of glacial acetic acid was added to react at room temperature for 4-8 h; then 300-600 μL of 12 M acetic acid solution was added to the reaction solution, and after ultrasonic mixing, the mixture was reacted at 70-100 °C for 24 h. After the reaction, the product was washed three times with tetrahydrofuran and ethanol respectively, and the precipitate was collected by centrifugation at 5000-8000 rpm for 5 min, and then dried in vacuum at 60-80 °C for 12-24 h to obtain a powdered UiO-66-(OH)2@COF-OCH3 composite material.
[0009] (4) Preparation of solid phase microextraction fiber coating using UiO-66-(OH)2@COF-OCH3 composite material First, the stainless steel fiber was ultrasonically cleaned with deionized water and ethanol respectively, and then one end (2-4 cm) of the stainless steel fiber was immersed in aqua regia for etching for 6-10 min, and then ultrasonically washed with deionized water and ethanol again after being taken out; then the cleaned etched end of the stainless steel fiber was vertically inserted into the organic silicone sealant, first rotated slowly and then pulled out quickly, and then moved into a centrifuge tube containing UiO-66-(OH)2@COF-OCH3 composite material powder and slowly rotated 2-3 times to make the fiber surface evenly coated. The stainless steel fiber coated with the composite material was placed in a 100 ℃ oven for curing for 3-5 h to obtain a solid phase microextraction fiber based on MOF@COF composite material. Before the fiber is used for extraction, it needs to be aged at 200-250 ℃ in the gas chromatography injection port for 2-4 h to remove volatile impurities.
[0010] The present invention firstly utilizes a solvothermal reaction to prepare a dihydroxyl-functionalized UiO-66-(OH)2 (MOF), and then uses a dual ligand-assisted strategy to amino-functionalize the MOF using polyethyleneimine and polyvinylpyrrolidone, thereby providing a basis for the effective heterogeneous nucleation of imine-bonded COF on its surface; the amino-functionalized UiO-66-(OH)2 is then added to a precursor solution of COF-OCH3 to prepare a core-shell structured UiO-66-(OH)2@COF-OCH3 composite material; finally, the composite material is coated onto an etched stainless steel fiber by an adhesive method to prepare a dual-functionalized MOF@COF coated solid phase microextraction fiber.
[0011] The MOF@COF composite material prepared by the present invention has a core-shell structure. Therefore, in order to avoid the inability to form a core-shell structure due to homogeneous nucleation of COF in the preparation of the composite material, the amount of COF monomer added needs to be strictly controlled. On the basis of ensuring heterogeneous nucleation on the MOF surface, the thickness of the COF shell layer can be controlled by changing the amount of COF monomer added, thereby improving the enrichment performance of the target object.
[0012] The main advantages of the present invention are: (1) The coated fiber prepared by the present invention has specific selectivity and good selectivity for halogenated persistent organic pollutants such as polybrominated diphenyl ethers, organochlorine pesticides, and hydroxylated polychlorinated biphenyls, and can specifically enrich such target substances, thereby improving the detection sensitivity of the combined method; (2) The UiO-66-(OH)2@COF-OCH3 composite coating material prepared by the present invention has a large specific surface area, good hydrophobicity and hierarchical porous structure. At the same time, it contains rich bifunctional groups (hydroxyl, methoxy) and π electronic structure, which enables it to produce multiple interactions such as hydrogen bonds, halogen bonds, π-π interactions, and hydrophobic interactions with active sites such as bromine, oxygen atoms, and benzene rings contained in the target. The coated fiber is used for SPME extraction of trace PBDEs in actual water samples and combined with GC-MS detection to achieve high-sensitivity and high-selectivity rapid analysis of pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to further illustrate the above and other advantages and features of the present invention, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The accompanying drawings only illustrate typical examples of the present invention.
[0014] Figure 1 This is the transmission electron microscopy image of the UiO-66-(OH)2@COF-OCH3 composite material; Figure 2 The scanning electron micrographs of the etched stainless steel fiber and the UiO-66-(OH)2@COF-OCH3 coated fiber; Figure 3 N2 adsorption-desorption isotherms of UiO-66-(OH)2@COF-OCH3 fiber coating; Figure 4 Selected ion chromatogram of environmental water samples. Black line: blank lake water sample; red line: spiked lake water sample, spike concentration: 10 ng L -1 ; Blue line: spiked lake water sample, spike concentration: 100 ng L -1 The chromatographic peaks in the figure correspond to the PBDEs mixture (BDE-28, BDE-47, BDE-100, BDE-99, BDE-154, BDE-153). DETAILED DESCRIPTION
[0015] The technical solution of the present invention is further described below by specific examples. The following examples are illustrative rather than restrictive, and the protection scope of the present invention cannot be limited by the following examples.
[0016] Example 1 (1) Preparation of UiO-66-(OH)2: 34 mg of 2,5-dihydroxyterephthalic acid and 40 mg of ZrCl4 were added to 10 mL of N,N-dimethylformamide and ultrasonically dissolved, and 3 mL of glacial acetic acid was added as a catalyst. The mixed solution was transferred to a 25 mL polytetrafluoroethylene-lined autoclave and reacted at 120 °C for 24 h. The product was then washed with ethanol six times, and the precipitate was collected by centrifugation at 8000 rpm for 5 min and vacuum dried at 60 °C overnight to obtain UiO-66-(OH)2.
[0017] (2) Surface amino functionalization treatment of UiO-66-(OH)2: 100 mg of UiO-66-(OH)2 was weighed and placed in a round-bottom flask containing 25 mL of ethanol and ultrasonicated for 1 h to make it evenly dispersed. 5 mL of an ethanol mixed solution of polyethyleneimine (100 mg / mL) and polyvinylpyrrolidone (100 mg / mL) was slowly added dropwise under stirring. After the addition was completed, it was stirred at room temperature for 12 h. The amino-functionalized UiO-66-(OH)2 product was then washed four times with ethanol, and the precipitate was collected by centrifugation at 8000 rpm for 5 min and dried in vacuum at 60 °C for 12 h.
[0018] (3) Preparation of UiO-66-(OH)2@COF-OCH3 composite material: 20 mg of amino-functionalized UiO-66-(OH)2, 2.8 mg of 2,5-dimethoxyterephthalaldehyde, and 2.3 mg of 1,3,5-tri(4-aminophenyl)benzene were added into a 6 mL round-bottom flask containing a mixed solvent of n-butanol and o-dichlorobenzene (v:v=1:1) and dissolved by ultrasonication. Then, 100 μL of glacial acetic acid was added to the mixed solution and reacted at room temperature for 4 h. Then, 400 μL of 12 M acetic acid solution was added to the reaction solution, and the mixture was ultrasonically mixed and reacted at 80 °C for 24 h. After the reaction, the product was washed with tetrahydrofuran and ethanol three times each, and the precipitate was collected by centrifugation at 8000 rpm for 5 min and dried in vacuo at 60 °C for 24 h to obtain a powdered UiO-66-(OH)2@COF-OCH3 composite material.
[0019] (4) Preparation of solid phase microextraction fiber based on UiO-66-(OH)2@COF-OCH3 composite material: First, ultrasonically clean the stainless steel fiber with deionized water and ethanol respectively, then immerse one end of the stainless steel fiber (3 cm) in aqua regia for etching for 10 min, take it out and ultrasonically wash it again with deionized water and ethanol; then vertically insert the etched end of the stainless steel fiber into the organic silicone sealant, rotate it slowly first and then pull it out quickly, and move it into a centrifuge tube containing UiO-66-(OH)2@COF-OCH3 composite material powder and rotate it slowly for 2 circles to make the surface of the etched end of the fiber evenly coated. The stainless steel fiber coated with the composite material was placed in a 100 °C oven for curing for 3 h to obtain the MOF@COF composite material solid phase microextraction fiber. Before being used for extraction, the fiber needs to be aged at 250 °C in the gas chromatography injection port for 1 h to remove volatile impurities.
[0020] Figure 1 This is a transmission electron microscopy image of the UiO-66-(OH)2@COF-OCH3 fiber coating material; it can be seen from the figure that the prepared composite material is a core-shell structure, and the thickness of the COF shell is 45.5 nm.
[0021] Figure 2 This is a scanning electron microscope image of UiO-66-(OH)2@COF-OCH3 stainless steel fiber and its coating; Figure 2 Figure a is a scanning electron microscope image of stainless steel fiber after aqua regia etching. Figure 2 Figure b is a scanning electron microscope image of the fiber after coating; by comparing the two images, it can be clearly seen that the UiO-66-(OH)2@COF-OCH3 coating (34.5 μm) has been evenly coated on the surface of the stainless steel fiber.
[0022] Figure 3 The N2 adsorption-desorption isotherm of UiO-66-(OH)2@COF-OCH3 fiber coating. It can be seen from the figure that it is a type IV isotherm, and the specific surface area of the coating material is 972.67 m 2 / g. The large specific surface area can provide more adsorption sites for the fiber coating, thereby improving the enrichment capacity of the analyte.
[0023] Example 2 In order to verify the enrichment performance of the UiO-66-(OH)2@COF-OCH3 composite framework material coated fiber for polybrominated diphenyl ethers, the coated fiber prepared in Example 1 was used for solid phase microextraction of PBDEs, and GC-MS was used to detect trace PBDEs in complex samples. The specific extraction and detection conditions were as follows: The results showed that the HPLC-MS / MS analysis showed that the HPLC-MS / MS analysis was effective for the detection of chromatographic residues in situ. The results showed that the HPLC-MS / MS analysis showed that the HPLC-MS / MS analysis was effective for the detection of situ hybridization. Under the set chromatographic conditions (capillary column (30 m×0.25 mm id×0.25 μm); carrier gas: high purity He; flow rate: constant flow, 1.0 mL / min; injection mode: splitless injection; injection port temperature: 280 °C; heating program: initial temperature 110 °C for 1 min, heating to 210 °C at a rate of 20 °C / min, holding for 1 min, and then heating to 280 °C at a rate of 10 °C / min, holding for 10 min; mass spectrometry conditions: interface temperature: 250 °C; solvent delay: 6 min; ion source: EI source; ionization energy: 70 eV; ion source temperature: 230 °C; SPME extraction conditions were optimized using full scan mode (Scan), mass scanning range (m / z): 50-750 amu; quantitative analysis was performed using selected ion detection mode (SIM)), and the optimal SPME extraction conditions (extraction temperature: 85 °C, extraction time: 45 min, desorption temperature: 280 ℃, desorption time was 7min, extraction stirring rate was 1200rpm, NaCl content was 0%), SPME-GC-MS was used to enrich and detect PBDEs in actual lake water samples. The detection method had a low detection limit (0.0026-0.034ng L -1 ).
[0024] Figure 4 The selected ion chromatogram of lake water samples measured in SIM mode. The spiked recoveries of the six PBDEs at two spiked concentrations were 79.0-117.4%, which met the detection requirements of GC-MS.
[0025] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing a solid phase microextraction fiber based on a dual-functional MOF@COF composite material, characterized in that: The following steps are involved: (1) Preparation of dihydroxy-functionalized UiO-66-(OH)2: 29.7-49.5 mg of 2,5-dihydroxyterephthalic acid and 34.9-93.5 mg of MCl4 (M = Zr, Hf, Th) were added to N,N-dimethylformamide for ultrasonic dissolution, and glacial acetic acid was added as a catalyst. The mixed solution was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 100-140 °C for 24 h. The obtained product was then washed with ethanol, collected by centrifugation, and vacuum dried overnight to obtain UiO-66-(OH)2; (2) Surface amino functionalization of UiO-66-(OH)2: UiO-66-(OH)2 was added to 25 mL of ethanol and dispersed evenly by ultrasonication. 5 mL of a mixed ethanol solution of polyethyleneimine and polyvinylpyrrolidone was slowly added dropwise under stirring. The mixture was magnetically stirred at room temperature for 12-24 h. The resulting solid product was then washed with ethanol, collected by centrifugation, and vacuum dried overnight to obtain amino-functionalized UiO-66-(OH)2. (3) Preparation of UiO-66-(OH)2@COF-OCH3 composite material: 5-35 mg of amino-functionalized UiO-66-(OH)2, 1.2-4.6 mg of 2,5-dimethoxyterephthalaldehyde, and 1.4-5.6 mg of 1,3,5-tri(4-aminophenyl)benzene were added to a mixed solvent of n-butanol and o-dichlorobenzene and dissolved by ultrasonication. Then, glacial acetic acid was added to the mixed solution and reacted at room temperature for 4-8 h. Then, a certain amount of 12 M acetic acid solution was added to the reaction solution, and the mixture was ultrasonically mixed and reacted at 70-100 °C for 24 h. After the reaction, the product was washed three times with tetrahydrofuran and ethanol respectively, collected by centrifugation, and then vacuum dried for 12-24 h to obtain a powdered UiO-66-(OH)2@COF-OCH3 composite material. (4) Preparation of UiO-66-(OH)2@COF-OCH3 composite solid phase microextraction fiber: First, the stainless steel fiber was ultrasonically cleaned with deionized water and ethanol respectively. Then, one end of the stainless steel fiber was immersed in aqua regia for etching. After taking it out, it was ultrasonically cleaned again with deionized water and ethanol. Then, the etched end of the stainless steel fiber was vertically inserted into the organic silicone sealant. It was first slowly rotated and then quickly pulled out and transferred into a centrifuge tube containing UiO-66-(OH)2@COF-OCH3 composite material powder and slowly rotated for 2-3 times to make it evenly coated. The stainless steel fiber coated with the composite material was placed in a 100 °C oven for curing to obtain the MOF@COF composite material solid phase microextraction fiber.
2. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: The volume of N,N-dimethylformamide used in step (1) is 5-15 mL, and the volume of glacial acetic acid is 1.5-4.5 mL; the prepared MOF is any one of UiO-66(Zr)-(OH)2, UiO-66(Hf)-(OH)2, and UiO-66(Th)-(OH)2.
3. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: In step (2), the concentration of the ethanol dispersion of UiO-66-(OH)2 is 3-5 mg / mL; the concentrations of both ligands in the ethanol mixed solution of polyethyleneimine and polyvinylpyrrolidone are 70-120 mg / mL.
4. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: In step (3), the volume ratio of n-butanol to o-dichlorobenzene is 1:1, and the total volume is 4-8 mL.
5. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: In step (3), 80-120 μL of glacial acetic acid is added at room temperature, and after the reaction is completed, 300-600 μL of 12 M acetic acid solution is added.
6. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: In step (4), the etching temperature of the stainless steel fiber is room temperature, and the etching time is 6-10 min; the fiber is cured in an oven at 100° C. for 3-5 h.
7. The method for preparing a dual-functional MOF@COF composite solid phase microextraction fiber according to claim 1, characterized in that: In steps (1) to (3), the centrifugal speed is 5000-8000 rpm, the centrifugal time is 4-8 min, and the vacuum drying temperature is 60-80 °C.
8. MOF@COF composite material solid phase microextraction fiber prepared according to the preparation method according to any one of claims 1 to 7.
9. Use of the MOF@COF composite material solid phase microextraction fiber according to claim 8 in the enrichment of polybrominated diphenyl ethers, organochlorine pesticides, and hydroxylated polychlorinated biphenyl organic pollutants.
10. The use according to claim 8, characterized in that: Before being used for extraction, the fiber needs to be aged in the gas chromatography injection port to remove volatile impurities; the aging temperature of the gas chromatography injection port fiber is 200-250°C and the aging time is 2-4 h.
Citation Information
Patent Citations
Preparation of MOF (at) COF core-shell composite material and application of MOF (at) COF core-shell composite material as solid-phase extraction adsorbent
CN114994199A
Stable defect MOF (at) COF material and preparation method and application thereof
CN118527127A