Magnetic composite material and preparation method and application thereof
The magnetic beads are bonded to the catalytic material through binders, stabilizers and buffers, and the catalyst recovery difficulties and shedding problems are solved through high-pressure and low-temperature treatment, achieving efficient catalyst recovery and degradation effects, ensuring the adsorption of the catalyst and catalytic activity.
Patent Information
- Application Number
- CN202411175845.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, catalyst recycling is difficult and easy to fall off, which affects the degradation effect. The catalyst bonds to magnetic materials with poor results, resulting in the risk of secondary pollution.
The magnetic beads are bonded to the catalytic material by using binders, stabilizers and buffers. The molecular bonds are enhanced by high-pressure and low-temperature freezing treatment to ensure the tight bond between the catalyst and the magnetic beads and avoid falling off.
The efficient recovery and degradation of the catalyst is achieved, the adsorption and catalytic activity of the catalyst are ensured, the recovery rate is more than 98.7%, and the degradation rate of mycotoxins in food reaches more than 90%.
Smart Images

Figure BDA0005010695330000091 
Figure BDA0005010695330000092 
Figure BDA0005010695330000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic material preparation, in particular to a magnetic composite material and a preparation method and application thereof. Background Art
[0002] At present, semiconductor photocatalytic oxidation technology uses visible light or ultraviolet light to degrade organic matter in the environment into water and carbon dioxide, and has broad application prospects in air purification, sterilization and deodorization, wastewater treatment, etc. However, the problem of catalyst recovery has not been well solved so far. If a large amount of catalyst residues are left after recovery, it will cause secondary pollution.
[0003] Composite catalytic materials and magnetic materials can not only achieve the recovery and recycling of catalysts, but also will not reduce the adsorption and catalytic activity of catalysts. It is an effective means to solve the above problems. However, the composite materials prepared in the prior art usually have poor bonding between catalytic materials and magnetic materials, are easy to fall off, and magnetic materials may coat the composite catalyst, which directly affects the recovery and degradation effect of catalytic materials. Summary of the invention
[0004] In order to solve the defects in the prior art, the present invention provides a magnetic composite material and a preparation method and application thereof, which improves the bonding performance of the catalytic material and the magnetic material and avoids falling off, so as to ensure the recovery rate and degradation effect.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a magnetic composite material, comprising the following steps:
[0007] mixing magnetic beads, a binder and a stabilizer to obtain mixed magnetic beads;
[0008] Catalytic materials and buffer solutions are added to the mixed magnetic beads to react, and solids are taken out after the reaction, frozen under the conditions of 2000-2500 bar pressure and -196° C., and taken out after the pressure is released.
[0009] Preferably, the binder is ethyl α-cyanoacrylate.
[0010] Preferably, the mass ratio of the magnetic beads to the binder is 5 to 20:1.
[0011] Preferably, the stabilizer is Tween 20 or Tween 66.
[0012] More preferably, the stabilizer is Tween 20.
[0013] Preferably, the catalytic material is gC 3 N4 / TiO 2 Composite materials.
[0014] Preferably, the mass ratio of the magnetic beads to the catalytic material is 1:5-10.
[0015] Preferably, the buffer is sodium barbital-hydrochloric acid buffer.
[0016] Preferably, the pH of the buffer solution is 7.5-8.5.
[0017] Preferably, the reaction temperature for adding the catalytic material and the buffer solution to the mixed magnetic beads is 100° C. and the reaction time is 4 hours.
[0018] Preferably, the solid is firstly cleaned and dried, and then subjected to high pressure and low temperature freezing treatment at a pressure of 2000 to 2500 bar and -196°C.
[0019] Preferably, the freezing time is 20 to 25 seconds.
[0020] In a second aspect, the present invention provides a magnetic composite material prepared by the above preparation method.
[0021] In a third aspect, the present invention provides an application of the magnetic composite material in degrading fungi in food.
[0022] Preferably, the food is selected from one or more of corn, wheat and rice.
[0023] Preferably, the fungus is selected from one or more of aflatoxin B1, zearalenone, and deoxynivalenol.
[0024] Preferably, the mass ratio of the grain to the magnetic composite material is 1000:1.
[0025] The beneficial effects of the present invention are:
[0026] The present invention allows magnetic beads and catalytic materials to be bonded by means of a binder, a stabilizer and a buffer. The binder allows the catalytic material to be completely attached to the surface of the magnetic beads, ensuring full contact with the degraded material during degradation and ensuring degradation efficiency. The stabilizer can adjust the viscosity of the binder so that the binder can be better attached to the surface of the magnetic beads. The buffer can reduce the increase in the fugacity of the binder due to the influence of temperature during the bonding reaction and maintain the stable activity of the binder. The solid obtained after the reaction needs to be subjected to high-pressure and low-temperature freezing treatment. After instantaneous pressure release, the water in the bioadhesive is completely released, the polymer structure of the binder is made more compact and orderly, the generation of molecular bonds is promoted, the hydrophobic interaction and the intermolecular hydrogen bond are enhanced, the electrostatic interaction is weakened, the molecular bond is strengthened, the catalyst and the magnetic beads are more closely combined, the catalyst will not be completely separated under ordinary mechanical stirring, and the recovery rate is guaranteed.
[0027] The magnetic composite material prepared by the present invention can be applied to grains of different crops and has a good recovery rate. When applied to a small amount of grain (less than 10 kg), it can achieve 100% recovery. When applied to a large amount of grain (more than 10 kg), it can basically guarantee a recovery rate of more than 98.7%. The recovery rate of the actual warehouse test is also more than 96%.
[0028] The magnetic composite material prepared by the invention has a good effect on the degradation of crop fungi, and the degradation rates of aflatoxin B1, zearalenone, deoxynivalenol and the like are all above 90%. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific implementation methods.
[0030] In order to avoid the problem that the catalytic material and the magnetic material in the prepared magnetic composite material have poor bonding performance and are easy to fall off, thereby affecting the recovery rate and degradation effect of the catalytic material, the present invention provides a method for preparing the magnetic composite material, comprising the following steps:
[0031] mixing magnetic beads, a binder and a stabilizer to obtain mixed magnetic beads;
[0032] Catalytic materials and buffer solutions are added to the mixed magnetic beads to react, and solids are taken out after the reaction, frozen under the conditions of 2000-2500 bar pressure and -196° C., and taken out after the pressure is released.
[0033] In the preparation method of the present invention, the magnetic beads and the catalytic material are subjected to a bonding reaction through an intermediary (a binder, a stabilizer and a buffer solution), wherein the catalytic material can be completely attached to the surface of the magnetic beads through the bonding effect of the binder, thereby ensuring full contact with the degraded material during degradation and ensuring degradation efficiency; the stabilizer can adjust the viscosity of the binder so that the binder can be better attached to the surface of the magnetic beads; the buffer solution can reduce the increase in the fugacity of the binder due to the influence of temperature during the bonding reaction and maintain the stable activity of the binder; the solid obtained after the reaction is then subjected to a high-pressure and low-temperature freezing treatment, and after instantaneous pressure release, the water in the bioadhesive is completely released, the polymer structure of the binder is made more compact and orderly, the formation of molecular bonds is promoted, the hydrophobic interaction and the intermolecular hydrogen bond are enhanced, the electrostatic interaction is weakened, the molecular bond is strengthened, the catalyst and the magnetic beads are more closely combined, and they will not be completely separated under ordinary mechanical stirring, thereby ensuring their recovery rate.
[0034] In some embodiments of the present invention, the preparation method of the hybrid magnetic beads is: the magnetic beads are first mixed with a binder, so that the binder is evenly wrapped on the magnetic beads, and then soaked in a stabilizer. In this embodiment, the binder is first evenly wrapped on the nano-scale magnetic beads, and then placed in a stabilizer. The stabilizer can adjust the viscosity of the binder on the one hand, and on the other hand, it can be used as a stabilizer for the binder, so that the binder can better adhere to the surface of the magnetic beads, which is more conducive to the subsequent steps of compounding. In another embodiment of the present invention, the preparation method of the hybrid magnetic beads is: the magnetic beads are first soaked in a stabilizer, and then a binder is added for mixing. In this embodiment, the magnetic beads are first soaked in a stabilizer. On the one hand, the stabilizer can adjust the viscosity of the subsequent addition of the binder, and on the other hand, the impurities on the surface of the magnetic beads can be washed away, and then the binder is added to achieve the bonding of the magnetic beads. The hybrid magnetic beads obtained by the above two methods of preparing hybrid magnetic beads have the same effect.
[0035] The binder of the present invention is ethyl α-cyanoacrylate, which is used to bond the magnetic beads and the catalytic material. The binder is non-toxic and harmless, and is inexpensive. When applied to the degradation process of food crops against fungi, it will not affect the degradation efficiency. In the present invention, the mass ratio of the magnetic beads: binder is 5 to 20:1. Exemplarily, the mass ratio of the magnetic beads: binder is any one of 5:1, 10:1, 20:1, or a value between the two.
[0036] The stabilizer of the present invention is Tween 20 or Tween 66, preferably Tween 20. The present invention does not limit the amount of the stabilizer, as long as it can immerse the magnetic beads. The stabilizer has three functions: first, it can adjust the viscosity of the binder; second, it can serve as a stabilizer for the binder to provide a stable environment so that the binder can better adhere to the surface of the magnetic beads; and third, it can wash away the residual chemical attachments on the surface of the magnetic beads to ensure better adhesion between the magnetic beads and the catalytic material.
[0037] In an embodiment of the present invention, the catalytic material is gC 3 N 4 / TiO 2 The present invention is to gC 3 N 4 / TiO 2 The preparation process of the catalytic material is not limited, and any method can obtain gC 3 N 4 / TiO 2 Catalytic materials can use the preparation method of the magnetic composite material of the present invention. In some embodiments of the present invention, the gC 3 N 4 / TiO 2 The preparation process of the catalytic material is as follows:
[0038] (1) Preparation of gC 3 N 4 : Mix melamine and ammonium chloride and calcine to obtain;
[0039] (2) Preparation of gC 3 N 4 / TiO 2 Catalytic material: TiO 2 Dissolve in alkaline solution, homogenize and mix with gC 3 N 4 The mixture is heated to react, and after the reaction, the solid is taken out and calcined to obtain the product.
[0040] In the present invention, the magnetic beads: gC 3 N 4 / TiO 2 The mass ratio of the catalytic material is 1:5-10.
[0041] The present invention mixes magnetic beads and gC 3 N 4 / TiO 2 The reaction temperature of the catalytic material is 100℃ and the reaction time is 4h. Due to the high temperature reaction, gC 3 N 4 / TiO 2 The adhesive is completely attached to the binder, but high temperature will affect the activity of the binder. Therefore, the present invention adds a buffer to the reaction system to reduce the fugacity of the binder increased by high temperature, so that the adhesive can still maintain stable activity in a high temperature environment. In some embodiments of the present invention, the buffer is sodium barbital-hydrochloric acid buffer. In some embodiments of the present invention, the pH of the buffer is 7.5 to 8.5, which will affect the adsorption effect of the catalytic material after exceeding the range.
[0042] Furthermore, in the present invention, after the solids are taken out, they are first cleaned and dried, and then subjected to high-pressure and low-temperature freezing treatment. The drying can be any drying form in the art, such as natural air drying, oven drying, etc.
[0043] The present invention finally uses high-pressure and low-temperature freezing conditions (2000-2500 bar pressure, -196°C freezing) to treat the reactants, so that after instantaneous pressure release, the water in the adhesive is completely released, making the adhesive polymer structure more compact and orderly, promoting the formation of molecular bonds, enhancing hydrophobic interactions and intermolecular hydrogen bonds, and weakening electrostatic interactions. Furthermore, the freezing time described in the present invention is 20-25 seconds.
[0044] In a second aspect, the present invention provides a magnetic composite material prepared by the above preparation method.
[0045] In a third aspect, the present invention proposes an application of the magnetic composite material in degrading fungi in food.
[0046] In some embodiments of the present invention, the food is selected from one or more of corn, wheat and rice.
[0047] In some embodiments of the present invention, the fungus is selected from one or more of aflatoxin B1, zearalenone, and deoxynivalenol.
[0048] In some embodiments of the present invention, the mass ratio of the grain to the magnetic composite material is 1000:1.
[0049] The above is a detailed description of the present invention. The following are examples of the present invention. All raw materials involved in the examples that are not specified are from commercially available high-grade purity.
[0050] Example 1
[0051] The preparation method of the magnetic composite material of this embodiment comprises the following steps:
[0052] S1. Preparation of gC 3 N 4 / TiO 2 Catalytic materials
[0053] 20 g of melamine and 4 g of ammonium chloride were weighed and introduced into a crucible for mechanical mixing. The mixture was placed in a muffle furnace and slowly heated to 550 °C at a heating rate of 10 °C / min. After calcination for 4 hours, the mixture was naturally cooled to room temperature and mechanically ground into powder to obtain flake gC 3 N 4 ; Weigh TiO 2 Dissolve 50g in 500mL of 5mol / L sodium hydroxide solution, homogenize with ultrasound for 20 minutes, and then add the prepared gC 3 N4 and TiO 2 The solution mixture was transferred to a round-bottom flask, which was connected to a condensing reflux device. The flask was heated for 4 hours, the solids at the bottom were taken out, rinsed with distilled water and dried, and then placed in a muffle furnace and slowly heated (10°C / min) to 400°C and fired for 1 hour. After being taken out, it was cooled to room temperature and mechanically ground into powder to obtain gC 3 N 4 / TiO 2 Catalytic materials.
[0054] S2. Preparation of Nanomagnetic Beads / gC 3 N 4 / TiO 2 Magnetic composite materials:
[0055] (1) Weigh 5 g of nano-scale magnetic beads, add ethyl α-cyanoacrylate (the mass ratio of nano-scale magnetic beads to ethyl α-cyanoacrylate is 5:1), and mix mechanically to make the ethyl α-cyanoacrylate evenly coated on the nano-scale magnetic beads, and immerse the nano-scale magnetic beads in Tween 20 for 4 hours to obtain mixed magnetic beads;
[0056] (2) Add the gC prepared in S1 to the magnetic beads of the mixture 3 N 4 / TiO 2 Catalytic material (nano-magnetic beads: gC 3 N 4 / TiO 2 The mass ratio of the catalytic material is 1:5), mixed and poured into a high-temperature reactor, added with sodium barbital-hydrochloric acid buffer (pH 8) and soaked at 100°C for 4 hours, then cooled to room temperature, the solid was taken out, rinsed with Tween 20, naturally air-dried and placed in a high-pressure freezer (pressure 2000 bar, temperature -196°C, maintained for 25 seconds), and then the pressure was released instantly to completely release the water in the bioadhesive, so that the polymer structure of the adhesive is more compact and orderly, and the solid obtained by using a grinder to make powder is the nanomagnetic bead / gC 3 N 4 / TiO 2 Magnetic composite materials.
[0057] Example 2
[0058] The same as Example 1, except that in step (2) of S2, the conditions of the high pressure freezer are: pressure 2500 bar, temperature -196°C, and hold for 20 seconds.
[0059] Example 3
[0060] S1. Preparation of gC 3 N 4 / TiO 2Catalytic material: same as in Example 1.
[0061] S2. Preparation of Nanomagnetic Beads / gC 3 N 4 / TiO 2 Magnetic composite materials:
[0062] (1) Weigh 5 g of nano-scale magnetic beads, completely immerse the nano-scale magnetic beads in Tween 20 for 4 h, add ethyl α-cyanoacrylate (the mass ratio of nano-scale magnetic beads to ethyl α-cyanoacrylate is 10:1), and mechanically mix to obtain a mixture of magnetic beads;
[0063] (2) Add the gC prepared in S1 to the magnetic beads of the mixture 3 N 4 / TiO 2 Catalytic material (nano-magnetic beads: gC 3 N 4 / TiO 2 The mass ratio of the catalytic material is 1:5), and after mixing, it is poured into a high-temperature reactor, and sodium barbital-hydrochloric acid buffer (pH 8) is added to soak and react at 100°C for 4 hours until it is cooled to room temperature and then soaked for another 4 hours. The solid is taken out, rinsed with Tween 20, and placed in a high-pressure freezer (pressure 2500 bar, temperature -196°C, maintained for 20 seconds) after natural air drying, and then the pressure is released instantly to completely release the water in the bioadhesive, so that the polymer structure of the adhesive is more compact and orderly. After taking it out, a grinder is used to make a powder to obtain the solid nanomagnetic beads.
[0064] / gC 3 N 4 / TiO 2 Magnetic composite materials.
[0065] Example 4
[0066] S1. Preparation of gC 3 N 4 / TiO 2 Catalytic material: same as in Example 1.
[0067] S2. Preparation of Nanomagnetic Beads / gC 3 N 4 / TiO 2 Magnetic composite materials
[0068] Weigh 5 g of nano-scale magnetic beads, soak them completely in Tween 20 for 4 h, add ethyl α-cyanoacrylate (the mass ratio of nano-scale magnetic beads to ethyl α-cyanoacrylate is 20:1), and mix them mechanically to obtain mixed magnetic beads;
[0069] Add the gC prepared in step (1) to the magnetic beads in the mixture 3N 4 / TiO 2 Catalytic material (nano-magnetic beads: gC 3 N 4 / TiO 2 The mass ratio of the catalytic material is 1:10), and then the mixture is poured into a high-temperature reactor, and barbital sodium-hydrochloric acid buffer (pH 8) is added to soak and react at 100°C for 4 hours until it is cooled to room temperature, and then the solid is taken out, rinsed with Tween 20, and then rinsed with ultrapure water, dried in an oven at 60°C, and placed in a high-pressure freezer (pressure 2000 bar, temperature -196°C, maintained for 25s), and then the pressure is released instantly to completely release the water in the bioadhesive, so that the polymer structure of the adhesive is more compact and orderly, and the solid obtained by using a grinder to make powder is the nanomagnetic bead / gC 3 N 4 / TiO 2 Magnetic composite materials.
[0070] Example 5
[0071] Same as Example 1, except that in step (2) of S2, the pH of the sodium barbital-hydrochloric acid buffer solution is 7.5.
[0072] Example 6
[0073] Same as Example 1, except that in step (2) of S2, the pH of the sodium barbital-hydrochloric acid buffer solution is 8.5.
[0074] Comparative Example 1
[0075] The same as Example 1, except that Tween is not added in step (1) of S2.
[0076] Comparative Example 2
[0077] The same as Example 1, except that no sodium barbital-hydrochloric acid buffer solution is added in step (2) of S2.
[0078] Comparative Example 3
[0079] The same as Example 1, except that in step (2) of S2, no high-pressure freezer is used for high-pressure and low-temperature treatment (pressure 2000 bar, temperature -196°C, maintained for 25 seconds).
[0080] Effect Example 1 Test of the Combination Performance of Catalytic Material and Magnetic Material in Magnetic Composite Material
[0081] Experimental process: The magnetic composite material prepared in Example 1 and Comparative Examples 1 to 3 is mixed with glass beads, and stirred thoroughly using a blender to simulate the situation of the composite material in a grain pile. The glass beads are then sieved out, and the magnetic substance is adsorbed with an iron magnet. The remainder is the catalytic material. The amount of material that falls off after stirring in the grain pile is calculated, thereby detecting the bonding performance of the composite material and the magnetic substance.
[0082] Experimental conditions: 0.1 g, 1 g, and 10 g of the magnetic composite material prepared in Example 1 and Comparative Examples 1 to 3 were added to 100 g, 1 kg, and 10 kg of glass beads, respectively, and the test was carried out under the conditions of simulating the temperatures of 15°C, 20°C, and 25°C in the granary and stirring times of 30 min, 60 min, and 120 min.
[0083] Experimental results: The test results of Example 1 are shown in Table 1, the test results of Comparative Example 1 are shown in Table 2, the test results of Comparative Example 2 are shown in Table 3, and the test results of Comparative Example 3 are shown in Table 4.
[0084] Table 1. Test results of magnetic composite material bonding performance of Example 1
[0085]
[0086] Conclusion: It can be seen from Table 1 that in the test of adding 0.1g of the magnetic composite material of Example 1 to 100g of glass beads, there is no shedding phenomenon of the catalytic material under the conditions of several temperatures and stirring times; in the test of adding 1g of the magnetic composite material of Example 1 to 1kg of glass beads, the maximum shedding rate does not exceed 2‰; in the test of adding 10g of the magnetic composite material of Example 1 to 10kg of glass beads, the shedding effect can be controlled within 1‰.
[0087] Table 2. Test results of magnetic composite material bonding performance of comparative example 1
[0088]
[0089]
[0090] Conclusion: From Table 2, it can be seen that when 0.1g of the magnetic composite material of Comparative Example 1 was added to 100g of glass beads, the shedding phenomenon occurred after stirring for 60min, and the maximum shedding rate reached 21%; when 1g of the magnetic composite material of Comparative Example 1 was added to 1kg of glass beads, the shedding rate was 8.9% to 24.9% after stirring for 30-120min; when 10g of the magnetic composite material of Comparative Example 1 was added to 10kg of glass beads, the shedding rate was 17.9% to 26.1%. That is, the magnetic composite material obtained in Comparative Example 1 has an obvious shedding effect, which reflects the important role of the stabilizer in the bonding of magnetic beads and catalytic materials in the preparation of magnetic composite materials.
[0091] Table 3. Test results of magnetic composite material bonding performance of comparative example 2
[0092]
[0093]
[0094] Conclusion: From Table 3, it can be seen that in the test of adding 0.1g of the magnetic composite material of Comparative Example 2 to 100g of glass beads, the composite material did not fall off; in the test of adding 1g of the magnetic composite material of Comparative Example 1 to 1kg of glass beads, the composite material began to fall off at a stirring time of 30-120min; in the test of adding 10g of the magnetic composite material of Comparative Example 2 to 10kg of glass beads, the composite material also fell off at a stirring time of 30-120min. That is, the magnetic composite material prepared in Comparative Example 2 has an obvious shedding effect, which reflects the effect of the buffer solution on the adhesion of the magnetic beads and the catalytic material in the process of preparing the magnetic composite material.
[0095] Table 4. Test results of magnetic composite material bonding performance of comparative example 3
[0096]
[0097]
[0098] Conclusion: It can be seen from Table 4 that in all experimental processes, the shedding rate of the magnetic composite material prepared in Comparative Example 3 was above 60%, and the shedding effect was extremely obvious, indicating that high-pressure and low-temperature treatment of the material during the preparation process can make the adhesive polymerization structure more compact and orderly, promote the formation of molecular bonds, enhance hydrophobic interactions and intermolecular hydrogen bonds, and improve the binding force between magnetic beads and catalytic materials.
[0099] Effect Example 2: Test on the recovery amount of magnetic composite materials and degradation effect on fungal toxins
[0100] Experimental Design:
[0101] 1. Mix the magnetic composite material and grain:
[0102] 0.1 g, 1 g, 10 g, 100 g, and 1000 g of the magnetic composite material prepared in Example 1 were added to 100 g, 1 kg, 10 kg, 100 kg, and 1 t of test grains (corn, wheat, and rice were used as experimental objects in this effect example), respectively. A 1 m × 1 m × 1 m area (approximately 1 t of grain) was demarcated in the real warehouse, and 1000 g of the above-mentioned magnetic composite material was added for a real warehouse test. The samples were manually mixed (100 kg and 1 t samples were mixed with a shovel), and after mixing, they were irradiated with a 50 w UVC lamp for 5 min, manually stirred, and irradiated with a 50 w UVC lamp for 5 min, and this was repeated 5 times, and allowed to stand for 24 h to allow full degradation.
[0103] 2. Separation of magnetic composite materials:
[0104] Electromagnetic iron rods are used to adsorb the magnetic composite material in the grain pile. Grain piles of 10kg, 100kg, and 1t need to be stirred and adsorbed at the same time to separate the magnetic composite material from the grain pile. The mass of the separated magnetic catalyst is weighed separately to detect the recovery amount.
[0105] 3. Test the degradation effect on fungal toxins:
[0106] (1) Sampling: 100g and 1kg of magnetic composite materials were all sampled using a hammer cyclone mill and passed through a 60-mesh sieve; 10kg of magnetic composite materials were divided into 1kg using a bell-tripper sample divider and sampled using a hammer cyclone mill and passed through a 60-mesh sieve; 100kg and 1t of magnetic composite materials were respectively sampled from the upper layer, middle layer and lower layer, 1kg each, mixed using a mixer, divided into 1kg using a bell-tripper sample divider and sampled using a hammer cyclone mill and passed through a 60-mesh sieve; a sampler was used in a real warehouse, and the 5-point plum blossom method was adopted to sample 500g of each point of the upper layer, middle layer and lower layer, mixed using a mixer, divided into 1kg using a bell-tripper sample divider and sampled using a hammer cyclone mill and passed through a 60-mesh sieve.
[0107] (2) Determination: Aflatoxin B1, zearalenone, and deoxynivalenol were determined in corn; zearalenone and deoxynivalenol were determined in wheat; and aflatoxin B1 was determined in rice. GB 5009.22-2016 (third method photochemical derivatization method), GB 5009.209 (first method), and GB 5009.111 (second method) were used for detection, and the results are shown in Table 5.
[0108] Table 5. Recovery amount of magnetic composite material and degradation effect on fungal toxins in Example 1
[0109]
[0110] As can be seen from Table 5, the magnetic composite material prepared by the present invention can be applied to the grains of different crops, and has a good recovery rate. When applied to a small amount of grain (less than 10kg), it can achieve 100% recovery. When applied to a large amount of grain (more than 10kg), it can basically guarantee a recovery rate of more than 98.7%, and the recovery rate of the actual warehouse test is also more than 96%. The magnetic composite material prepared by the present invention also has a good effect on the degradation of crop fungi, and has a good degradation rate for aflatoxin B1, zearalenone, deoxynivalenol, etc.
[0111] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a magnetic composite material, characterized in that: The following steps are involved: mixing magnetic beads, a binder and a stabilizer to obtain mixed magnetic beads; Catalytic materials and buffer solutions are added to the mixed magnetic beads to react, and solids are taken out after the reaction, frozen under the conditions of 2000-2500 bar pressure and -196° C., and taken out after the pressure is released.
2. The preparation method according to claim 1, characterized in that: The binder is ethyl α-cyanoacrylate.
3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the magnetic beads to the binder is 5 to 20:
1.
4. The preparation method according to claim 1, characterized in that: The stabilizer is Tween 20 or Tween 66.
5. The preparation method according to claim 1, characterized in that: The buffer is sodium barbital-hydrochloric acid buffer.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the magnetic beads to the catalytic material is 1:5-10.
7. The preparation method according to claim 1, characterized in that: The reaction temperature for adding the catalytic material and the buffer solution to the mixed magnetic beads is 100° C. and the reaction time is 4 hours.
8. A magnetic composite material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the magnetic composite material according to claim 8 in degrading fungi in food.
10. The use according to claim 9, characterized in that: The fungus is selected from one or more of aflatoxin B1, zearalenone, and deoxynivalenol.