Preparation method of monatomic-based catalytic ceramic membrane as well as product and application of monatomic-based catalytic ceramic membrane

Loading single-atom catalysts inside ceramic membrane pores addresses inefficiencies in traditional membranes and single-atom catalyst recovery, enabling efficient and cost-effective pollutant removal with high flux and broad applicability.

CN119056440AActive Publication Date: 2024-12-03JINGDEZHEN CERAMIC UNIV

Patent Information

Application Number
CN202411176478.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Traditional catalytic ceramic membranes have limited specific surface area and catalytic active sites due to large transition metal nanopowders, leading to inefficient removal of new pollutants, while single-atom catalysts face challenges in recovery, mass transfer, and high application costs, limiting their large-scale use in wastewater treatment.

Method used

A method to load single-atom catalysts (Mn, Co, Cu, Fe, Ni, Ag) inside ceramic membrane pores, using a precursor solution and vacuum drying, ensuring even distribution and high active site utilization, without forming a separate separation layer.

Benefits of technology

The method achieves efficient pollutant removal under high flux conditions with enhanced catalytic performance, low preparation costs, and wide applicability, utilizing ceramic membrane nano-space and single-atom catalysts' advantages, achieving 100% degradation efficiency of pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056440A_ABST
    Figure CN119056440A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a monatomic-based catalytic ceramic membrane as well as a product and application of the monatomic-based catalytic ceramic membrane, the ceramic membrane is soaked in a monatomic catalyst precursor solution until a saturated state is reached, and the monatomic precursor solution is subjected to vacuum drying under the constraint condition of a nano confinement space of membrane pores to obtain the monatomic-based catalytic ceramic membrane. And forming a complex of metal and a carbon-nitrogen precursor in membrane pores, and then performing high-temperature calcination treatment in a protective atmosphere to obtain the monatomic metal-loaded catalytic ceramic membrane. According to the invention, the monatomic (Mn, Co, Cu, Fe, Ni, Ag and the like) catalyst is loaded in the membrane pores of the ceramic membrane to prepare the monatomic-based catalytic ceramic membrane, so that the excellent catalytic performance of the monatomic catalyst and the nano space of the membrane pores of the ceramic membrane are fully utilized, and an oxidizing agent is coupled / activated; and efficient removal of new pollutants under the condition of high permeation flux is realized under the nano confinement catalytic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of membrane-based confined catalytic water treatment, and in particular to a method for preparing a single-atom-based catalytic ceramic membrane, and a product and application thereof. Background Art

[0002] New pollutants exist in all kinds of sewage and wastewater, which seriously threaten the ecological environment and human health. Catalytic ceramic membranes coupled with advanced oxidation processes are considered to be a feasible technology for removing new pollutants in sewage and wastewater because of their high redox potential, ability to generate strong oxidizing reactive oxygen species (ROS), nano-confined catalytic effect and high pollutant removal efficiency. However, the preparation of traditional catalytic ceramic membranes is to load transition metal nanopowders inside the membrane pores of the ceramic membrane. For example, the prepared ceramic membrane is immersed in a mixed solution including metal precursor salts and structure directing agents by an impregnation method, and then dried and treated with low-temperature plasma to obtain a catalytic ceramic membrane. Due to the relatively large particle size of transition metal nanopowders, the specific surface area of ​​the catalytic ceramic membrane is relatively small and the catalytic active sites are relatively few, resulting in limited reaction efficiency between ROS and new pollutant molecules, which seriously limits the removal efficiency of new pollutants in sewage and wastewater.

[0003] Compared with traditional transition metal nanoparticle catalysts, single-atom catalysts have adjustable electronic structures, nearly 100% atomic utilization, more active sites and atomic-level dispersion, so they have excellent catalytic removal of new pollutants. However, in the application process of single-atom catalysts, there are still problems such as difficulty in catalyst recovery, limited mass transfer between ROS and pollutant molecules, and inability to achieve continuous catalytic reactions, which leads to high application costs and limits their large-scale application in the field of new pollutant removal.

[0004] To this end, the prior art has developed a technology that uses a single-atom catalyst coupled with a ceramic membrane to solve the above-mentioned bottleneck problem. For example, by loading a single-atom catalyst on a ceramic substrate membrane to prepare a catalytic membrane, the problem of recycling the single-atom catalyst is solved. However, since the single-atom catalyst has strong hydrophobicity, it is difficult for it to enter the interior of the membrane pores, resulting in the existing single-atom-based catalytic ceramic membranes still being prepared by a conventional dip-coating suspension method, that is, first preparing a single-atom catalyst, and then preparing the single-atom catalyst into a coating suspension, and preparing a catalytic ceramic membrane by a dip-coating process. This method ultimately forms a single-atom catalytic film layer on the ceramic membrane substrate, resulting in problems such as uneven pore size distribution of the catalytic membrane, small membrane flux, and high membrane preparation cost. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a single-atom-based catalytic ceramic membrane, by loading a single-atom (Mn, Co, Cu, Fe, Ni, Ag, etc.) catalyst inside the membrane pores of the ceramic membrane to prepare the single-atom-based catalytic ceramic membrane, thereby making full use of the excellent catalytic performance of the single-atom catalyst and the nanospace of the ceramic membrane pores, and achieving efficient removal of new pollutants under high permeation flux conditions under the nano-confined catalytic effect. Another purpose of the present invention is to provide a product prepared by the preparation method of the above-mentioned single-atom-based catalytic ceramic membrane and its application.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] The present invention provides a method for preparing a single-atom-based catalytic ceramic membrane, comprising the following steps:

[0008] (1) Preparation of single-atom-based metal catalyst precursor solution

[0009] (1-1) adding melamine to dimethyl sulfoxide (DMSO) in a mass volume ratio of melamine: cyanuric acid: dimethyl sulfoxide = 1 g: 1 g: 20-40 mL, stirring and mixing to dissolve to obtain a solution A; adding cyanuric acid to dimethyl sulfoxide (DMSO), stirring and mixing to dissolve to obtain a solution B;

[0010] (1-2) taking a metal nitrate solution having a concentration of 10 to 20 g / L based on the mass of the metal, taking two equal amounts of the A solution and the B solution; adding the metal nitrate solution to the A solution and stirring evenly in a volume ratio of nitrate solution to A solution = 1:2 to 5, and then adding the B solution and stirring evenly to obtain a single atom-based metal catalyst precursor solution;

[0011] (2) Preparation of single-atom-based catalytic ceramic membranes

[0012] The ceramic membrane is placed in the precursor solution, and vacuum pressure is used to allow the ceramic membrane to fully absorb the precursor solution until it is saturated. After the ceramic membrane is taken out after the first vacuum drying, the excess single-atom metal catalyst particles on the surface of the ceramic membrane are washed with a dimethyl sulfoxide (DMSO) solution, and then a second vacuum drying is performed to obtain a completely dry ceramic membrane loaded with single atoms. The membrane is then calcined at a temperature of 400 to 600°C under a protective atmosphere and kept warm for 3 to 6 hours to obtain a single-atom-based catalytic ceramic membrane.

[0013] Furthermore, the metal nitrate described in the present invention is one of iron nitrate (Fe(NO3)3·9H2O), cobalt nitrate (Co(NO3)2·6H2O), nickel nitrate (Ni(NO3)2), manganese nitrate (Mn(NO3)2·6H2O), silver nitrate (AgNO3), and copper nitrate (Cu(NO3)2).

[0014] Furthermore, in step (2) of the present invention, the vacuum extraction is carried out at a vacuum degree of 0.5-1.0 MPa for 20-30 min. The first vacuum drying is carried out at a vacuum degree of 0.8 MPa and a temperature of 60-100° C. for 2-4 h; the second vacuum drying is carried out at a vacuum degree of 0.9 MPa and a temperature of 80-100° C. for 3-5 h.

[0015] In the above scheme, the average pore size of the ceramic membrane of the present invention is 50 to 500 nm.

[0016] Another object of the present invention is achieved by the following technical solutions:

[0017] The product is made by using the preparation method of the above-mentioned single-atom-based catalytic ceramic membrane.

[0018] The application of the single-atom-based catalytic ceramic membrane product of the present invention is as follows: the single-atom-based catalytic ceramic membrane product is used to couple / activate the oxidant continuous flow process to degrade new pollutants in ultrapure water. When the concentration of the new pollutants is 1 to 10 mg / L, the molar ratio of oxidant: new pollutant = 1: 0.02 to 0.10, and the membrane flux is 100 to 150 LMH, the degradation efficiency of the new pollutants during the continuous catalytic reaction process of 5 to 7 hours is 100%.

[0019] In the above scheme, the oxidant in the application of the present invention is persulfate, hydrogen peroxide, ozone, or peracetic acid. The new pollutants are bisphenol A, ibuprofen, sulfamethoxazole, paracetamol, carbamazepine and other drugs and care products and endocrine disruptors.

[0020] The present invention has the following beneficial effects:

[0021] (1) The present invention loads the single-atom catalyst into the membrane pores of the ceramic membrane, making full use of the extremely excellent catalytic performance of the single-atom catalyst and the nano-space of the ceramic membrane pores. Since the single-atom catalyst is fixed inside the ceramic membrane pores, the single-atom catalyst will not flow with the water when water flows through, thereby effectively solving the bottleneck problem of the recovery and practical utilization of the single-atom catalyst powder; at the same time, the single-atom catalyst does not form a new separation layer, and the permeation resistance is small. The high specific surface area of ​​the ceramic membrane is effectively utilized to greatly increase the reaction active sites of the catalytic ceramic membrane and its utilization efficiency and the yield of ROS, breaking through the trade-off between the permeation flux of the catalytic ceramic membrane and the catalytic removal efficiency of pollutants, and realizing the efficient removal of new pollutants under high permeation flux conditions.

[0022] (2) The present invention requires low preparation cost and good universality. Different types of single-atom catalysts can be loaded inside the membrane pores of the ceramic membrane, and the preparation process is simple, which is conducive to promoting the large-scale application of single-atom catalysts and catalytic ceramic membranes.

[0023] (3) The single-atom-based catalytic ceramic membrane of the present invention couples / activates oxidants such as persulfate, hydrogen peroxide, ozone and peracetic acid, which can efficiently remove new pollutants in wastewater. During the catalytic reaction, the ceramic membrane pores loaded with single-atom catalysts can provide nano-confined catalytic space, effectively improving the yield and utilization efficiency of ROS, effectively alleviating membrane pollution while increasing the contact probability between ROS and new pollutant molecules, and achieving efficient removal of new pollutants in wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:

[0025] Figure 1 This is a scanning electron microscope photograph of the surface and cross section of the single-atom manganese-based catalytic ceramic membrane prepared in Example 1 of the present invention;

[0026] Figure 2 These are scanning electron microscope photos of the surface and cross-section of the single-atom iron-based catalytic ceramic membrane prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0027] Embodiment 1:

[0028] This embodiment provides a method for preparing a single atom-based catalytic ceramic membrane, and the steps are as follows:

[0029] (1) Preparation of single-atom catalyst precursor solution

[0030] (1-1) adding melamine to dimethyl sulfoxide (DMSO) at a mass volume ratio of melamine: cyanuric acid: dimethyl sulfoxide = 1 g: 1 g: 30 mL, stirring and mixing (speed of 250 r / min, time of 20 min) to dissolve, to obtain solution A; adding cyanuric acid to dimethyl sulfoxide (DMSO) and stirring and mixing (speed of 250 r / min, time of 20 min) to dissolve, to obtain solution B;

[0031] (1-2) taking a manganese nitrate solution having a concentration of 20 g / L in terms of metal mass, taking two equal amounts of solution A and solution B; adding the manganese nitrate solution to solution A according to a volume ratio of manganese nitrate solution: solution A = 1:3, stirring evenly (at a speed of 250 r / min for 30 min), and then continuing to add solution B and stirring and mixing (at a speed of 250 r / min for 30 min), to obtain a single atom manganese catalyst precursor solution;

[0032] (2) Preparation of single-atom-based catalytic ceramic membranes

[0033] A ceramic membrane with an average pore size of 200 nm was placed in the above-mentioned precursor solution, and vacuum pressure was used at a vacuum degree of 0.6 MPa for 30 minutes to allow the ceramic membrane to fully absorb the precursor solution until saturated. The membrane was then taken out and placed in a vacuum drying oven (vacuum degree 0.8 MPa, temperature 70°C) for a vacuum drying for 3 hours. Excess catalyst particles on the surface of the ceramic membrane were washed with a dimethyl sulfoxide (DMSO) solution, and then placed in a vacuum drying oven (vacuum degree 0.9 MPa, temperature 90°C) for a second vacuum drying for 5 hours to obtain a completely dried ceramic membrane loaded with single atoms, which was then placed in a tubular furnace for calcination at 550°C under a N2 protective atmosphere and kept warm for 4 hours to obtain a single-atom manganese-based catalytic ceramic membrane (see Figure 1 ).

[0034] Embodiment 2:

[0035] The present embodiment is a method for preparing a single-atom-based catalytic ceramic membrane, which is different from the first embodiment in that:

[0036] 1. In step (1), the mass volume ratio of melamine: cyanuric acid: dimethyl sulfoxide = 1 g: 1 g: 25 mL;

[0037] 2. In step (2), the metal nitrate is ferric nitrate, and the concentration of the ferric nitrate solution is 15 g / L based on the mass of the metal;

[0038] 3. The average pore size of the ceramic membrane in step (2) is 100 nm; the calcination temperature is 500° C. and the temperature is kept for 3 hours;

[0039] 4. The prepared film is a single-atom iron-based catalytic ceramic membrane (see Figure 2 ).

[0040] like Figure 1 and Figure 2 As shown, in the single-atom-based catalytic ceramic membrane prepared in an embodiment of the present invention, the single-atom catalyst is loaded on the surface and cross-section of the ceramic membrane without forming a separate separation membrane layer; and the single-atom catalyst is evenly distributed inside the membrane pores without blocking the pores and increasing the permeation resistance.

[0041] Embodiment three:

[0042] The application of the single-atom manganese-based catalytic ceramic membrane in this embodiment is as follows: the single-atom manganese-based catalytic ceramic membrane prepared in Example 1 is used to activate the permonosulfate continuous flow process to degrade bisphenol A in ultrapure water. When the permonosulfate concentration is 1.0 mM, the bisphenol A concentration is 8 mg / L, and the membrane flux is 130 LMH, the degradation efficiency of bisphenol A in the continuous catalytic reaction for 5 hours is 100%.

[0043] Embodiment 4:

[0044] The application of the single-atom-based catalytic ceramic membrane in this embodiment is as follows: the single-atom iron-based catalytic ceramic membrane prepared in Example 2 is used to activate the hydrogen peroxide continuous flow process to degrade carbamazepine in ultrapure water. When the hydrogen peroxide concentration is 0.6 mM, the carbamazepine concentration is 10 mg / L, and the membrane flux is 120 LMH, the degradation efficiency of carbamazepine during the continuous 6-h catalytic reaction process is 100%.

Claims

1. A method for preparing a single-atom-based catalytic ceramic membrane, characterized in that The following steps are involved: (1) Preparation of single-atom-based metal catalyst precursor solution (1-1) adding melamine to dimethyl sulfoxide in a mass volume ratio of melamine: cyanuric acid: dimethyl sulfoxide = 1 g: 1 g: 20-40 mL, stirring and mixing to dissolve to obtain a solution A; adding cyanuric acid to dimethyl sulfoxide, stirring and mixing to dissolve to obtain a solution B; (1-2) taking a metal nitrate solution having a concentration of 10 to 20 g / L based on the mass of the metal, taking two equal amounts of the A solution and the B solution; adding the metal nitrate solution to the A solution and stirring evenly in a volume ratio of nitrate solution to A solution = 1:2 to 5, and then adding the B solution and stirring evenly to obtain a single atom-based metal catalyst precursor solution; (2) Preparation of single-atom-based catalytic ceramic membranes The ceramic membrane is placed in the precursor solution, and vacuum pressure is used to allow the ceramic membrane to fully absorb the precursor solution until it is saturated. After the ceramic membrane is taken out after the first vacuum drying, the excess single-atom metal catalyst particles on the surface of the ceramic membrane are washed off with a dimethyl sulfoxide solution, and then a second vacuum drying is performed to obtain a completely dry ceramic membrane loaded with single atoms. The membrane is then calcined at a temperature of 400 to 600°C under a protective atmosphere and kept warm for 3 to 6 hours to obtain a single-atom-based catalytic ceramic membrane.

2. The method for preparing a single-atom-based catalytic ceramic membrane according to claim 1, characterized in that: The metal nitrate is one of iron nitrate, cobalt nitrate, nickel nitrate, manganese nitrate, silver nitrate and copper nitrate.

3. The method for preparing a single-atom-based catalytic ceramic membrane according to claim 1, characterized in that: The vacuum extraction in step (2) is performed at a vacuum degree of 0.5 to 1.0 MPa for 20 to 30 minutes.

4. The method for preparing a single-atom-based catalytic ceramic membrane according to claim 1, characterized in that: In the step (2), the first vacuum drying is performed at a vacuum degree of 0.8 MPa and a temperature of 60 to 100° C. for 2 to 4 hours; the second vacuum drying is performed at a vacuum degree of 0.9 MPa and a temperature of 80 to 100° C. for 3 to 5 hours.

5. The method for preparing a single-atom-based catalytic ceramic membrane according to claim 1, characterized in that: The average pore size of the ceramic membrane is 50-500 nm.

6. A product obtained by the method for preparing a single-atom-based catalytic ceramic membrane according to any one of claims 1 to 5.

7. The use of the single-atom-based catalytic ceramic membrane product according to claim 6, characterized in that: The single-atom-based catalytic ceramic membrane product is used to couple / activate the oxidant continuous flow process to degrade new pollutants in ultrapure water. When the concentration of the new pollutants is 1-10 mg / L, the molar ratio of oxidant: new pollutant = 1: 0.02-0.10, and the membrane flux is 100-150 LMH, the degradation efficiency of the new pollutants during the continuous catalytic reaction process of 5-7 hours is 100%.

8. The use of the single-atom-based catalytic ceramic membrane product according to claim 7, characterized in that: The oxidant is persulfate, hydrogen peroxide, ozone, or peracetic acid.

9. The use of the single-atom-based catalytic ceramic membrane product according to claim 7, characterized in that: The new pollutants are bisphenol A, ibuprofen, sulfamethoxazole, paracetamol, and carbamazepine.

Citation Information

Patent Citations

  • Monatomic cobalt-doped carbon material confinement ceramic membrane as well as construction method and application thereof

    CN117282281A

  • Pollution-resistant composite modified ceramic membrane as well as preparation method and application thereof

    CN117599621A

  • Single atomic metal catalyst and carbon dioxide conversion system using the same

    US20230383426A1

Cited By

  • Preparation method and application of catalytic membrane based on monatomic iron-manganese oxide

    CN119488922A