Catalyst for preparing dimethyl 1, 4-cyclohexanedicarboxylate as well as preparation method and application of catalyst

A catalyst with a dispersed Pd and Ru on Al2O3 carrier addresses the high palladium content issue in DMCD production, achieving high conversion and selectivity rates with reduced costs and improved stability.

CN119056443APending Publication Date: 2024-12-03CHINA NAT PETROLEUM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410229530.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing industrial production of dimethyl 1,4-cyclohexanedicarboxylate (DMCD) using the dimethyl terephthalate (DMT) hydrogenation method faces challenges with high palladium content, high costs due to rising palladium prices, and the need for catalysts with high reactivity and stability under mild reaction conditions.

Method used

A catalyst with a highly dispersed eggshell structure of Pd and Ru on an Al2O3 carrier, where Pd accounts for 0.6-0.83 wt% and Ru for 0.04-0.08 wt%, prepared through a method involving impregnation and calcination, reduces palladium content while maintaining reaction activity and stability.

Benefits of technology

The catalyst achieves a conversion rate greater than 99.5% and selectivity greater than 93%, with reduced palladium content, lower operating costs, and improved stability, suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and discloses a catalyst for preparing dimethyl 1, 4-cyclohexanedicarboxylate as well as a preparation method and application of the catalyst. Pd and Ru serve as catalytic active metals and are loaded on the Al2O3 carrier in a high-dispersion manner to form an eggshell-shaped structure, Pd accounts for 0.6-0.83 wt% of the total content of the catalyst, and Ru accounts for 0.04-0.08 wt% of the total content of the catalyst. On the premise that reaction activity and stability are not affected, the content of precious metal is reduced, and cost reduction and efficiency improvement are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate and a preparation method and application thereof. Background Art

[0002] Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) is an important chemical raw material intermediate that can be used for polymer modification materials and can also be used for hydrogenation to produce 1,4-cyclohexanedimethanol (CHDM). CHDM is one of the important raw materials for high-performance, new environmentally friendly engineering plastics and packaging materials that have attracted great attention in the market in recent years. At present, the only industrial production method of DMCD is the dimethyl terephthalate (DMT) hydrogenation method. However, the DMT benzene ring hydrogenation reaction is very difficult, and effective catalytic active substances usually include metal elements such as Pd, Pt, Ru, and Ni. There are many influencing factors to consider in the hydrogenation process. It is necessary to ensure that the benzene ring is hydrogenated thoroughly and the benzene ring cannot be opened. The existing DMT hydrogenation industrial catalyst mostly chooses Pd as the active metal component, and the Pd content is as high as 2%. In recent years, the market price of Pd has been on the rise. In order to reduce project costs and processing costs, it is necessary to develop advanced catalyst technology with high reactivity, mild reaction conditions, and low precious metal content. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention provides a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate, a preparation method and application thereof, which reduces the content of precious metals while ensuring that the reaction activity and stability are not affected, thereby achieving cost reduction and efficiency improvement.

[0004] The above object of the present invention is achieved through the following technical solutions:

[0005] A catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate, wherein Pd and Ru as catalytically active metals are highly dispersedly loaded on an Al2O3 carrier to form an eggshell structure, wherein Pd accounts for 0.6-0.83wt% of the total content of the catalyst, and Ru accounts for 0.04-0.08wt%.

[0006] Preferably, Pd accounts for 0.81 wt% of the total content of the catalyst, and Ru accounts for 0.045 wt%.

[0007] The present invention also claims a method for preparing the above catalyst, the specific steps of which are as follows:

[0008] S1. Pretreatment of Al2O3 carrier: soaking Al2O3 pellet carrier in NaCl solution, taking it out and drying it in oven to obtain activated carrier;

[0009] S2. Preparation of an impregnation solution; anhydrous PdCl2 and RuCl3 were dissolved in NaCl solution as a solvent to prepare an impregnation solution;

[0010] S3. Impregnation load; the activated carrier obtained in step S1 is placed in a beaker, the impregnation solution prepared in step S2 is poured onto the activated carrier, the beaker is rotated at a constant speed so that the activated carrier is in uniform contact with the impregnation solution, adsorbed, and cleaned;

[0011] S4. Drying;

[0012] S5. Secondary impregnation loading; repeating step S3;

[0013] S6. Gradient drying; the impregnated catalytically active metal-loaded support was dried at 60 to 90 ° C for 3 to 4 h, and the solid support was dried at 110 to 130 ° C for 3 to 4 h;

[0014] S7. Calcination: Calcinate at 330-370°C for 5-7h to obtain the catalyst.

[0015] Furthermore, the volume ratio of the Al2O3 pellet carrier to the NaCl solution in step S1 is 0.5-1:1.5-3.

[0016] Furthermore, the Al2O3 pellet carrier in step S1 is a nano-Al2O3 pellet carrier.

[0017] Furthermore, the drying conditions in step S1 are 100-120° C. and drying time of 2-4 hours.

[0018] Furthermore, the concentration of the NaCl solution in step S1 is 0.03-0.07M.

[0019] Furthermore, the concentration of the NaCl solution in step S2 is 0.03-0.07M.

[0020] Furthermore, the impregnation solution in step S2 contains 0.003-0.007 g / mL of Ru and 0.018-0.019 g / mL of Pd.

[0021] Furthermore, the RuCl3 in step S2 is prepared by adding Ru at a content of 0.05 to 0.0516 wt%.

[0022] Furthermore, the PdCl2 in step S2 is prepared by adding Pd at a content of 0.4 to 0.0414 wt%.

[0023] Furthermore, in step S3, the volume ratio of the activated carrier to the impregnation liquid is 1:2 to 2.5.

[0024] Furthermore, the uniform rotation in step S3 is 25-50 r / min.

[0025] Furthermore, the adsorption time in step S3 is 1 to 2 hours, and the residual liquid is poured off after adsorption.

[0026] Furthermore, the cleaning in step S3 specifically includes: cleaning the carrier loaded with catalytically active metal with deionized water, and repeating the cleaning for multiple times.

[0027] Furthermore, the drying conditions in step S4 are specifically: solid drying at 100-120° C. for 3-4 hours.

[0028] The preparation of dimethyl 1,4-cyclohexanedicarboxylate adopts the DMT hydrogenation method, which requires the use of the above catalyst, wherein the catalyst is reduced by the following method.

[0029] DMT one-stage hydrogenation catalyst reduction: reduction pressure 0 ~ 1MPa, using hydrogen reduction, its purity is 99.99%, volume space velocity 1000 ~ 3000h -1 ,The programmed temperature conditions are: room temperature-30min-120℃, 30min-120℃, 60min-300℃, 240min-300℃, and then down to room temperature.

[0030] The present invention also claims to protect the use of the catalyst prepared by the above preparation method in catalyzing the hydrogenation of a 1,4-cyclohexanedicarboxylic acid dimethyl ester solution of DMT to prepare 1,4-cyclohexanedicarboxylic acid dimethyl ester.

[0031] Based on the total mass of the DMT 1,4-cyclohexanedicarboxylic acid dimethyl ester solution (hereinafter referred to as DMT solution), the mass concentration of the DMT is 10-50%, and 1,4-cyclohexanedicarboxylic acid dimethyl ester is used as a solvent for dissolving DMT; the temperature of the 1,4-cyclohexanedicarboxylic acid dimethyl ester solution catalyzing the hydrogenation reaction of DMT is 140-185° C., the hydrogen pressure is 8-12 MPa, the purity is 99.99%, and the liquid hourly space velocity of dimethyl terephthalate is 0.1-0.5 h -1 , the molar ratio of raw material hydrogen to oil is 70-250.

[0032] The beneficial effects of the present invention compared with the prior art are:

[0033] The present invention provides a method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate, wherein NaCl is used as a dissolving liquid to replace concentrated hydrochloric acid to fully dissolve the PdCl2 active component, and the impregnation process does not require continuous stir-frying and evaporation and dehydration at a certain temperature, thereby reducing labor intensity. After a certain period of loading, the impregnation liquid is filtered and sent to a drying process, and the catalyst is dried in a gradient manner to prepare the catalyst. The preparation method improves the stability and dispersibility of the active metal loading, the palladium content can be reduced to 0.8%, the conversion rate is greater than 99.5%, and the selectivity is greater than 93%. The prepared catalyst has excellent stability. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The present invention is described in detail below by specific examples, but the protection scope of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.

[0036] In the description of the present invention, it should be noted that the terms "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or component referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are only used for distinction, and cannot be understood as indicating or implying relative importance.

[0037] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0038] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.

[0039] Product analysis and data processing adopt the following methods and calculation methods:

[0040] A gas chromatograph (hydrogen flame detector, SE-54 chromatographic column) was used to detect the composition of the raw materials and products, and to calculate the reaction conversion rate and selectivity.

[0041] One stage hydrogenation reaction:

[0042] Conversion rate = (DMT content of raw material - DMT content of product) / DMT content of raw material * 100%

[0043] Selectivity = (DMCD content of product - DMCD content of raw material) / (DMT content of raw material - DMT content of product) * 100%

[0044] Example 1

[0045] A catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate, wherein Pd is highly dispersedly loaded on an Al2O3 carrier as a catalytically active metal to form an eggshell structure, wherein Pd accounts for 0.81wt% of the overall content of the catalyst.

[0046] The present invention also claims a method for preparing the above catalyst, the specific steps of which are as follows:

[0047] S1. Pretreatment of Al2O3 carrier: soaking Al2O3 pellet carrier in NaCl solution, taking it out and drying it in oven to obtain activated carrier;

[0048] S2. Preparation of an impregnation solution; anhydrous PdCl2 and RuCl3 were dissolved in NaCl solution as a solvent to prepare an impregnation solution;

[0049] S3. Impregnation load; the activated carrier obtained in step S1 is placed in a beaker, the impregnation solution prepared in step S2 is poured onto the activated carrier, the beaker is rotated at a constant speed so that the activated carrier is in uniform contact with the impregnation solution, adsorbed, and cleaned;

[0050] S4. Drying;

[0051] S5. Secondary impregnation loading; repeating step S3;

[0052] S6 gradient drying; the impregnated catalytically active metal carrier was dried at 80 ° C for 4h and solid dried at 120 ° C for 4 hours;

[0053] S7. Calcination: Calcinate at 350°C for 6 hours to obtain a catalyst.

[0054] The volume ratio of the Al2O3 pellet carrier to the NaCl solution in step S1 is 1:2.

[0055] The Al2O3 pellet carrier in step S1 is a nano-Al2O3 pellet carrier.

[0056] The drying conditions in step S1 are 110° C. and 3 hours.

[0057] The concentration of the NaCl solution in step S1 is 0.05M.

[0058] The concentration of the NaCl solution in step S2 is 0.05M.

[0059] The impregnation solution in step S2 contains 0.005 g / mL of Ru and 0.0185 g / mL of Pd.

[0060] The RuCl3 in step S2 is prepared by adding Ru at a content of 0.0508 wt%.

[0061] The PdCl2 in step S2 is prepared by adding Pd at a content of 0.407 wt%.

[0062] The volume ratio of the activated carrier to the impregnation liquid in step S3 is 1:2.

[0063] The uniform rotation speed in step S3 is 50 r / min.

[0064] The adsorption time in step S3 is 1 hour, and the residual liquid is poured off after adsorption.

[0065] The cleaning in step S3 specifically includes: cleaning the carrier loaded with catalytically active metal with deionized water, and repeating the cleaning for multiple times.

[0066] The drying conditions in step S4 are specifically: drying at 120° C. for 4 hours.

[0067] The catalyst prepared in Example 1 and the existing commercially available catalyst were tested for physical properties, and the test results are compared in Table 1.

[0068] Table 1. Catalyst index comparison table

[0069]

[0070] Example 2

[0071] Pd accounts for 0.80 wt% of the total content of the catalyst. Other contents are the same as those in Example 1.

[0072] Example 3

[0073] Pd accounts for 0.82 wt% of the total content of the catalyst. Other contents are the same as those in Example 1.

[0074] Example 4

[0075] Pd accounts for 0.83 wt% of the total content of the catalyst. Other contents are the same as those in Example 1.

[0076] Example 5

[0077] Pd accounts for 0.60 wt% of the total content of the catalyst. Other contents are the same as those in Example 1.

[0078] Example 6

[0079] Pd accounts for 0.72 wt% of the total content of the catalyst. Other contents are the same as those in Example 1.

[0080] Comparative Example 1.

[0081] Pretreatment of Al2O3 carrier: Take the Al2O3 small ball carrier, put it in a small stainless steel dish, dry it in an oven at 120℃ for 6 hours, and set aside.

[0082] Preparation of impregnation solution: Weigh anhydrous PdCl2, dissolve it with hydrochloric acid and NaCl deionized water, stir evenly, prepare PdCl2 solution, and set aside.

[0083] Impregnation process: weigh 10 grams of carrier and put it in a glass culture dish. Pour the above-prepared impregnation solution on the carrier in the culture dish and quickly stir it with a small spatula to mix it as evenly as possible. Place it in an oven (60°C) overnight to achieve stable loading.

[0084] Drying: Dry in an oven at 120°C for 6 hours.

[0085] Calcination: In a muffle furnace, set the temperature program to rise to 350°C for 2 hours and calcine for 6 hours to obtain a catalyst sample.

[0086] Pd accounts for 1 wt% of the total content of the catalyst.

[0087] Comparative Example 2

[0088] Pd accounts for 1.1 wt% of the total content of the catalyst. Other contents are the same as those in Comparative Example 1.

[0089] Comparative Example 3

[0090] Pd accounts for 1.2 wt% of the total content of the catalyst. Other contents are the same as those in Comparative Example 1.

[0091] Comparative Example 4

[0092] Pd accounts for 2.0 wt% of the total content of the catalyst. Other contents are the same as those in Comparative Example 1.

[0093] Determination of the porosity of the prepared catalyst

[0094] 100 particles of each catalyst prepared in Example 1, Example 2, and Example 3 were tested and the average particle size was 2.4 mm.

[0095] The calculated volume of each catalyst group = 4 / 3*(Π*R 3 )*100

[0096] =4 / 3*(3.14*0.12 3 )*100

[0097] =0.688cm 3

[0098] Each group of catalysts was weighed, and the average value was 0.61 g

[0099] The calculated catalyst apparent density is ρ = 0.61 / 0.688 = 0.887 g / cm 3

[0100] The tested catalyst bulk density ρ0 is 0.546 g / cm 3

[0101] Void ratio = (1-ρ0 / ρ)*100%

[0102] =(1-0.546 / 0.887)*100%

[0103] =38.44%.

[0104] 100 particles of catalysts prepared in Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested and found to have an average particle size of 2.6 mm.

[0105] The calculated volume of each catalyst group = 4 / 3*(Π*R 3 )*100

[0106] =4 / 3*(3.14*0.13 3 )*100

[0107] =0.9198cm 3

[0108] Each group of catalysts was weighed, and the average value was 1.0399 g

[0109] The calculated apparent density of the catalyst is ρ = 1.0399 / 0.9198 = 1.130 g / cm 3

[0110] The catalyst bulk density was tested to be ρ0 = 0.766 g / cm 3

[0111] Void ratio = (1-ρ0 / ρ)*100%

[0112] =(1-0.766 / 1.130)*100%

[0113] =32.21%.

[0114] The porosity of the catalysts prepared in Examples 1-3 is higher than that of the catalyst prepared in the comparative example.

[0115] Study on the service life of the catalyst prepared in Example 1

[0116] To further investigate its applicability for industrialization, a 500-hour long-term life evaluation was conducted in a hydrogenation evaluation device. The results showed that the average reaction conversion rate was 99.25% and the average selectivity was 93.22%, proving that the catalyst prepared in the embodiment of the present invention has good life stability.

[0117] The catalyst prepared in Example 1 was used in a hydrogenation evaluation device to conduct a temperature study on the application of the catalyst in the DMT first stage hydrogenation reaction.

[0118] At a reaction pressure of 8 MPa and a volume space velocity of 0.4 h -1 The influence of different reaction temperatures on the hydrogenation effect was investigated under the conditions of 1:1 hydrogen-to-oil molar ratio and 10% mass concentration of DMT solution as raw material. As shown in Table 2 below, as the reaction temperature decreases, the conversion rate remains unchanged and the selectivity can be increased by 2 to 3 percentage points, indicating that the catalyst can be used under lower temperature conditions, which is conducive to reducing production energy consumption. Compared with existing catalysts, the working temperature is lower and good conversion rate and selectivity can be guaranteed.

[0119] Table 2. Conversion rate and selectivity of the catalyst prepared in Example 1 at different reaction temperatures

[0120] Reaction temperature, °C Conversion rate, % Selectivity, % 205 99.8 91~92 195 99.7 92~93 185 99.6 93~94 175 99.7 93~94 165 99.8 94~95 155 98~99 94~95

[0121] Evaluation of scale-up trial production of catalysts prepared in Example 1 and Example 4

[0122] Two catalyst scale-up trials were carried out, and the industrial scale-up trials and evaluation results are shown in Table 3. The conditions for industrial mass production are met.

[0123] Table 3. Catalyst industrial scale-up trial production and evaluation results

[0124] catalyst Pd content, w% DMT conversion rate, % DMCD selectivity, % Trial production 1# 0.830 99.081 90.14 Trial production 2# 0.817 99.65 93.31

[0125] Application Example 1

[0126] The catalyst prepared in Example 1-6 was operated in a hydrogenation evaluation device at a reaction temperature of 165°C, a reaction pressure of 8 MPa, and a volume space velocity of 0.4 h -1 The results are shown in Table 4.

[0127] Table 4. Catalyst industrial production and evaluation results

[0128] Production batch Bulk density, g / ml Strength, N / grain Pd content, w% DMT conversion rate, % DMCD selectivity, % Example 6 0.539 70.4 0.72 99.70 93.12 Example 5 0.531 70.3 0.60 99.64 93.09 Example 4 0.529 70.6 0.83 99.77 93.31 Example 3 0.542 70.7 0.82 99.92 94.09 Example 2 0.544 70.0 0.80 99.79 93.10 Example 1 0.535 70.1 0.81 100.00 94.30

[0129] Application Example 2

[0130] The catalyst prepared in Example 1 was industrially scaled up and operated in a CHDM production unit at a reaction temperature of 135° C. The results are shown in Table 5.

[0131] Table 5. Catalyst industrial production and evaluation results

[0132] project Pd content, w% DMT conversion rate, % DMCD selectivity, % Industrial Agents 0.81 99.93 95.67

[0133] Application Comparative Example 1

[0134] The catalyst prepared in Comparative Examples 1-4 was run in a hydrogenation evaluation device at a reaction temperature of 210°C, a reaction pressure of 8 MPa, and a volume space velocity of 0.4 h -1 The results are shown in Table 6.

[0135] Table 6. Comparative Example Catalyst Industrial Production and Evaluation Results

[0136]

[0137]

[0138] The above-described embodiments are only preferred embodiments of the present invention, and are not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made to it without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention. Although the present invention has been described above with reference to the embodiments, various improvements can be made to it and the components thereof can be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no technical conflict, the various features in the embodiments disclosed in the present invention can be used in combination with each other in any way, and the fact that these combinations are not exhaustively described in this specification is only for the purpose of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate, characterized in that: Pd and Ru as catalytically active metals are highly dispersed and loaded on the Al2O3 carrier to form an eggshell structure, in which Pd accounts for 0.6-0.83wt% of the total content of the catalyst and Ru accounts for 0.04-0.08wt%.

2. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 1, characterized in that: The specific steps are as follows: S1. Pretreatment of Al2O3 carrier: soaking Al2O3 pellet carrier in NaCl solution, taking it out and drying it in oven to obtain activated carrier; S2. Preparation of an impregnation solution; anhydrous PdCl2 and RuCl3 were dissolved in NaCl solution as a solvent to prepare an impregnation solution; S3. Impregnation load; the activated carrier obtained in step S1 is placed in a beaker, the impregnation solution prepared in step S2 is poured onto the activated carrier, the beaker is rotated at a constant speed so that the activated carrier is in uniform contact with the impregnation solution, adsorbed, and cleaned; S4. Drying; S5. Secondary impregnation loading; repeating step S3; S6. Gradient drying; the impregnated catalytically active metal-loaded support was dried at 60 to 90 ° C for 3 to 4 h, and the solid support was dried at 110 to 130 ° C for 3 to 4 h; S7. Calcination: Calcinate at 330-370°C for 5-7h to obtain the catalyst.

3. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The volume ratio of the Al2O3 pellet carrier to the NaCl solution in step S1 is 0.5-1:1.5-3.

4. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The drying conditions in step S1 are 100-120° C. and 2-4 hours.

5. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The impregnation solution in step S2 contains 0.003-0.007 g / mL of Ru and 0.018-0.019 g / mL of Pd.

6. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The volume ratio of the activated carrier to the impregnation liquid in step S3 is 1:2 to 2.

5.

7. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The adsorption time in step S3 is 1 to 2 hours, and the residual liquid is poured off after adsorption.

8. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The cleaning in step S3 specifically includes: cleaning the carrier loaded with catalytically active metal with deionized water, and repeating the cleaning six times.

9. The method for preparing a catalyst for preparing dimethyl 1,4-cyclohexanedicarboxylate as claimed in claim 2, characterized in that: The drying conditions in step S4 are specifically: solid drying at 100-120° C. for 3-4 hours.

10. Use of the catalyst prepared by the preparation method according to any one of claims 2 to 9 in the preparation of dimethyl 1,4-cyclohexanedicarboxylate.