Oil film coated in-situ reduced noble metal catalyst, preparation method and application
Through the in-situ reduction method of oil film wrapping, the problems of low utilization rate of precious metals and large particle size in the preparation of precious metal catalysts are solved, and higher catalytic activity and simplified preparation process are achieved, thereby improving the dispersion and temperature stability of precious metals.
Patent Information
- Application Number
- CN202310646870.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-02
AI Technical Summary
The existing precious metal catalysts have low utilization rate and large particle size during the preparation process, resulting in low catalytic activity and require additional reduction and activation steps to increase cost and complexity.
The in-situ reduction method is adopted to wrap oil films, and the reduction agent and stabilizer are added to the impregnation liquid to form nano precious metal particles during the drying process, and the holes are blocked with high boiling point oily substances to avoid evaporation of the reducing agent, so as to achieve originality in the drying step. bit reduction simplifies the preparation process.
The dispersion and utilization of precious metals are improved, the particle size is reduced, the preparation process is simplified, and the activity and temperature stability of the catalyst are improved, avoiding additional reduction activation steps.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to an oil film-wrapped in-situ reduction noble metal catalyst, a preparation method and an application thereof, and belongs to the field of VOCs waste gas purification. Background Art
[0003] The current VOCs treatment technologies mainly include direct oxidation, adsorption, absorption, catalytic oxidation, biological methods, etc. Among the many technologies, various control technologies have their own advantages and disadvantages in terms of application scope and removal efficiency. Catalytic oxidation technology is one of the most promising and efficient chemical treatment technologies. It has the advantages of low-temperature catalytic activity (200-500°C), no secondary pollution (avoiding the formation of nitrogen oxides), high treatment efficiency (removal efficiency is mostly above 95%) and a wide range of applications. In catalytic oxidation technology, catalysts are the core technology. The catalysts currently used in industrial applications mainly use precious metals as active components and honeycomb ceramics or metal corrugated plates as the matrix. Since precious metal catalysts are expensive, it is necessary to increase the utilization rate of precious metals in catalysts, reduce the amount of precious metals used, and increase catalyst activity.
[0004] CN201310453379.7 discloses a catalyst for tail gas purification and a preparation method thereof, and provides a catalyst for tail gas purification and a preparation method thereof, the catalyst comprising an alumina carrier, cerium dioxide loaded on the alumina, and a noble metal active component loaded on the surface of the cerium dioxide. A precipitation hydrothermal method is used to prepare the alumina carrier and the cerium dioxide, and a hydrothermal in-situ reduction deposition method is used to load the noble metal active component. CeO2 and the noble metal species in the catalyst interact strongly, and the CeO2 carrier can produce more oxygen vacancies, activate oxygen molecules to convert into active oxygen species, and improve the catalytic oxidation activity. Alumina and cerium dioxide are dispersed and contacted with each other, and play a mutual barrier role, which can avoid sintering with pure cerium oxide as a carrier, and significantly improve the thermal stability of alumina at high temperatures.
[0005] CN201610281077.X discloses a catalyst for catalytic decomposition of formate to produce hydrogen at room temperature, and relates to a titanium dioxide nanorod-loaded palladium (Pd) nanoparticle catalyst for formate decomposition reaction. The patent document uses titanium dioxide nanorods as carriers, and loads nano Pd on the carrier surface through a surface-modified in-situ reduction method to obtain a loaded catalyst. The loaded catalyst for room temperature formate decomposition to produce hydrogen can achieve efficient catalytic decomposition of formate at room temperature, producing pure H2 without the presence of other gases. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides an oil film-wrapped in-situ reduced precious metal catalyst, a preparation method and an application thereof.
[0007] As one aspect of the present invention, it relates to an oil film wrapped in-situ reduction precious metal catalyst, wherein the oil film wrapped in-situ reduction precious metal catalyst comprises a carrier and nano precious metal particles loaded on the carrier, wherein the carrier is divided into a first carrier and a second carrier, the inner surface of the pores of the first carrier is coated with the second carrier, and the nano precious metal particles are distributed on the inner surface of the pores of the second carrier.
[0008] In a possible specific implementation manner, the porosity of the first carrier is 20% to 95%, the positive compressive strength of the carrier is greater than 0.5 MPa, and the side compressive strength is greater than 0.2 MPa.
[0009] It should be noted that, although a large porosity means good gas permeability, it may affect its strength. It is preferably 20% to 90%, preferably 60-95%, to take both strength and gas permeability into consideration.
[0010] In a possible specific implementation manner, the first carrier is honeycomb ceramic and / or honeycomb metal.
[0011] In a possible specific embodiment, the second carrier is one of TiO2, cerium-zirconium solid solution, γ-Al2O3 and ZSM-5 molecules, or any mixture thereof;
[0012] In a possible specific embodiment, the nano noble metal includes at least one of gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum.
[0013] As another aspect of the present invention, it relates to a method for preparing the above-mentioned oil film-wrapped in-situ reduced precious metal catalyst, the preparation method comprising the following steps:
[0014] S1: mixing the second carrier powder additive and the organic additive, and ball milling to obtain a coated catalyst slurry;
[0015] S2: coating the coated catalyst slurry of S1 onto the carrier, and then drying and calcining to obtain a catalyst carrier;
[0016] S3: Dissolve and mix the noble metal precursor, reducing agent, buffer and stabilizer in deionized water, and impregnate them onto the catalyst support of S2 by equal volume impregnation method, so that the impregnation liquid completely enters the micropores of the support, and then drip the coating agent to cover the surface of the support;
[0017] S4: placing the impregnated support obtained in S3 in a N2 atmosphere for reaction;
[0018] S5: slowly release N2 under the N2 atmosphere of S4 and dry;
[0019] S6: The dried carrier is placed in a muffle furnace for calcination to obtain an oil film-coated in-situ reduced precious metal catalyst.
[0020] In a possible specific embodiment, the encapsulating agent is an alkane oily encapsulating agent with a boiling point range of 120 to 290° C. or a water-insoluble organic substance within this boiling point range;
[0021] Preferred is n-decane, n-octane, n-dodecane or n-hexadecane.
[0022] In a possible specific embodiment, the organic auxiliary agent is one of alcohols, aldehydes, organic acids, and sodium borohydride;
[0023] The organic additive is used for the second carrier to improve the coating effect, and is preferably PEG or a leveling agent.
[0024] In a possible specific embodiment, the reducing agent is methanol or ethylene glycol.
[0025] In a possible specific embodiment, the stabilizer is a water-soluble polymer substance, preferably polyvinyl pyrrolidone, polyethylene glycol or F123.
[0026] In a possible specific embodiment, the buffer is a weak organic acid-organic acid salt system with a pH of 3 to 7, preferably citric acid-citrate, EDTA or polyacrylic acid-polyacrylic acid salt.
[0027] In a possible specific implementation manner, in the step S1, the ball milling time is 0.1 to 30 hours.
[0028] In a possible specific implementation manner, in step S4, the pressure of the N2 atmosphere is 0.18MPA-0.65MPa, the volume percentage of O2 is less than 1%, the reaction time is 2-4h, and the reaction temperature is 80-95°C.
[0029] In a possible specific implementation manner, in step S5, the drying is two-end drying, the first stage drying temperature is 120°C to 300°C, and the second stage drying temperature is 300°C.
[0030] In a possible specific implementation manner, in step S6, the baking temperature is 500-600° C., and the baking time is 2-4 hours.
[0031] As another aspect of the present invention, it relates to the use of the above-mentioned oil film-wrapped in-situ reduction precious metal catalyst or the oil film-wrapped in-situ reduction precious metal catalyst prepared by the above-mentioned preparation method in catalytic oxidation treatment of volatile organic compounds.
[0032] Based on the above technical solution, the beneficial effects of the present invention compared with the prior art are as follows:
[0033] The oil film-wrapped in-situ reduction noble metal catalyst of the present invention is conducive to the reduction reaction during the drying process because the reducing agent, stabilizer and buffer are added to the impregnation liquid, and nanoparticles are formed and attached to the carrier under the action of the stabilizer;
[0034] In addition, the oil film-wrapped in-situ reduction precious metal catalyst of the present invention has a layer of high-boiling-point oily substance attached to the outside of the carrier impregnated with the precious metal solution, forming an oil film to block the catalyst pore openings, and sealing the impregnation liquid in the carrier pores, which can prevent the low-boiling-point reducing agent from evaporating and overflowing, resulting in the reducing agent being completely evaporated when the temperature reaches the reduction temperature, making it difficult to complete the reduction of the precious metal, and most of the precious metal still exists in the ionic state, causing the ions to migrate and aggregate with the solvent, and the precious metal is unevenly distributed, and at the same time, it is not reduced and activated, and needs to be reduced and activated again in subsequent use;
[0035] In addition, the reduction process of the oil film-wrapped in-situ reduction of the precious metal catalyst described in the present invention occurs during the catalyst drying step, eliminating the need for a pre-reduction treatment process of the impregnation liquid.
[0036] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and claims. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited by the following embodiments.
[0038] Traditional methods for preparing precious metal catalysts include impregnation, pre-reduction impregnation, and co-impregnation. The precious metal catalysts obtained by these methods need to be reduced and activated using hydrogen or hydrazine hydrate before use. During the reduction process, the precious metals will aggregate to form larger particles, resulting in a low utilization rate of the precious metals.
[0039] The inventors of this case found in actual work that in-situ reduction can be achieved during the catalyst drying process to form particles with small particle size and uniform distribution, which effectively simplifies the preparation process of precious metal catalysts and improves the utilization rate of precious metals.
[0040] Based on the above objectives, in order to simplify the reduction process of precious metal catalysts, reduce the particle size of precious metals in the catalyst, improve the dispersion of precious metals, and thus improve the catalytic activity, the inventors of this case adopted the following technical solutions:
[0041] The present invention adopts a commonly used impregnation method to prepare the catalyst. After impregnation, the reducing agent is protected by attaching an oil film, and the active components are dispersed in the micropores of the carrier. The active components are reduced and activated while drying, and the reduced nano-precious metal particles generated by the reaction are directly loaded on the surface of the carrier pores. The carrier powder has abundant pores. Since the carrier powder is immersed in a precious metal precursor solution, the solute in the solution is distributed inside and outside the carrier pores, so the reduction reaction is also distributed inside and outside the carrier pores. The reduced metal particles are distributed on various surfaces inside and outside the carrier pores, which further improves the dispersion of the precious metal, thereby improving the activity and metal utilization rate of the obtained precious metal catalyst.
[0042] The Pt and Pd precursors are configured into a 0.5% to 2% solution (based on Pt and Pd single substances), and then methanol, citric acid, PVP and deionized water are added. The solution is then impregnated onto a pre-treated carrier. A layer of alkane oily coating agent (C8 to C16) with a boiling range of 120 to 290°C is then impregnated onto the carrier impregnated with the precious metal solution. The product is placed in a drying oven and reacted at 80 to 95°C for 2 to 4 hours under the protection of 0.4MPaN2 to reduce the precious metal to a single substance. The protective gas is slowly released to prevent violent volatilization from causing the surface layer to burst until it reaches normal pressure. N2 protection is continued, the temperature is raised to 120 to 300°C, and drying is continued for 4 hours to completely volatilize the reducing agent, water and oily coating agent. After drying, the product is placed in a muffle furnace at 500 to 600°C for calcination for 2 to 4 hours to crystallize the oxide additive to form the desired catalyst.
[0043] The present invention does not specifically limit the precious metal in the precious metal precursor, which may be Pt or Pd. The precious metal precursor is a Pt-containing compound or a Pd-containing compound, and the precious metal precursor aqueous solution is an aqueous solution containing a Pt compound or an aqueous solution containing a Pd compound.
[0044] The present invention does not particularly limit the method of ball milling, and ball milling can be performed in a ball mill. The ball milling time is, for example, 0.1 to 30 hours, preferably 0.5 to 3 hours.
[0045] In addition, the inventors of this case found that in the process of preparing nano precious metals, the precious metal particles produced by thermal reduction using methanol as a reducing agent are small in size and have better catalytic performance. The reduction reaction temperature is preferably 80-120°C, but the boiling point of methanol is 65°C. Under normal pressure, the reducing agent has completely volatilized before the reduction reaction temperature is reached. The present invention adopts an oil film plugging method. Under positive pressure nitrogen sealing conditions, the reaction system solution including the reducing agent is blocked in the carrier pores with an oil film, so that the reduction reaction is completed in the carrier pores, and the generated precious metal nanoparticles are uniformly adsorbed in the carrier pores. According to the saturated vapor pressure of methanol at 80°C, which is 180.667kPa and 120°C, the reaction system pressure is controlled between 0.18MPa and 0.65MPa.
[0046] Example
[0047] Source of raw materials or equipment:
[0048]
[0049]
[0050] Evaluation and analysis methods:
[0051] Analytical instrument: Agilent 8860 gas chromatograph with FID detector for quantitative analysis of reactants.
[0052] Containing 1000mg / m 3 Benzene-containing air was used as the evaluation gas source. Isothermal evaluation was performed on a fixed bed reactor with a reaction space velocity of 20,000 h -1 , conversion rate = (1-benzene content at the reaction outlet / benzene content at the reaction inlet) × 100%, T 90 It is the reaction temperature when the benzene conversion rate reaches 90%, unit is ℃.
[0053] Example 1
[0054] 0.44g of citric acid and 8.5g of PVP were dissolved in 40ml of deionized water, and 12.5ml of methanol, 48g of chloroplatinic acid solution with a platinum content of 2% and 12g of palladium chloride solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution with a total precious metal content of 10g / L; 120ml of deionized water was added to a mixed powder of 25g of γ-Al2O3 and 5g of cerium-zirconium solid solution, and ball milled at a speed of 400 rpm for 1 hour to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 25g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-decane was dripped to cover the catalyst surface, and the reaction was carried out at 80°C for 2 hours in a 0.4MPaN2 atmosphere. The catalyst was dried at 160°C under nitrogen protection and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a noble metal content of 1g / L.
[0055] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =192℃.
[0056] Comparative Example 1
[0057] 0.44g of citric acid and 8.5g of PVP were dissolved in 40ml of deionized water, and 12.5ml of methanol, 48g of chloroplatinic acid solution with a platinum content of 2% and 12g of palladium chloride solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution with a total precious metal content of 10g / L; 120ml of deionized water was added to a mixed powder of 25g of γ-Al2O3 and 5g of cerium-zirconium solid solution, and ball milled at a speed of 400 rpm for 1 hour to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 25g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, the reaction was carried out at 80°C for 2h in a 0.4MPaN2 atmosphere, dried at 160°C under nitrogen protection, and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a precious metal content of 1g / L.
[0058] The catalyst was not reactivated and evaluated. The evaluation results showed that 90 =358℃.
[0059] 5% H2 + 95% N2 was introduced and the catalyst was evaluated after activation at 200℃ for 1h. The evaluation results showed that benzene T 90 =264℃.
[0060] Example 2
[0061] 0.44g of citric acid and 8.5g of PVP were dissolved in 40ml of deionized water, and 12.5ml of methanol, 48g of chloroplatinic acid solution with a platinum content of 2% and 12g of palladium chloride solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution with a total precious metal content of 10g / L; 120ml of deionized water was added to a mixed powder of 25g of γ-Al2O3 and 5g of cerium-zirconium solid solution, and ball milled at a speed of 400 rpm for 1 hour to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 25g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-octane was dripped to cover the catalyst surface, and the reaction was carried out at 80°C for 2 hours in a 0.18MPaN2 atmosphere. The catalyst was dried at 160°C under nitrogen protection, dried at 120°C, and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a precious metal content of 1g / L.
[0062] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =196℃.
[0063] Example 3
[0064] 0.44g of citric acid and 8.5g of PVP were dissolved in 40ml of deionized water, and 12.5ml of methanol, 48g of chloroplatinic acid solution with a platinum content of 2% and 12g of palladium chloride solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution with a total precious metal content of 10g / L; 120ml of deionized water was added to a mixed powder of 25g of γ-Al2O3 and 5g of cerium-zirconium solid solution, and ball milled at a speed of 400 rpm for 1 hour to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 25g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-hexadecane was dripped to cover the catalyst surface, and the reaction was carried out at 120°C for 2 hours in a 0.65MPaN2 atmosphere. The catalyst was dried at 160°C under nitrogen protection, dried at 300°C, and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a precious metal content of 1 g / L.
[0065] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =192℃.
[0066] Example 4
[0067] 0.44g EDTA and 8.5g ammonium polyacrylate were dissolved in 40ml deionized water, and 12.5ml methanol, 48g platinum nitrate solution with a platinum content of 2% and 12g palladium nitrate solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution ① with a total precious metal content of 10g / L; 120ml deionized water was added to a mixed powder of 25g γ-Al2O3 and 5g cerium-zirconium solid solution, and the mixture was ball-milled at a speed of 400 rpm for 1 hour to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 25g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-decane was dripped to cover the catalyst surface, and the reaction was carried out at 85°C in a 0.4MPaN2 atmosphere for 2h. The catalyst was dried at 160°C under nitrogen protection and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a noble metal content of 1g / L.
[0068] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =174℃.
[0069] Example 5
[0070] 8.4g of ammonium polyacrylate and 3.6g of polyacrylic acid were dissolved in 40ml of deionized water, and 12.5ml of ethylene glycol, 48g of platinum nitrate solution with a platinum content of 2% and 12g of palladium nitrate solution with a palladium content of 2% were added to the solution, and the volume was adjusted to 120ml to form an impregnation solution ① with a total precious metal content of 10g / L; 50ml of deionized water was added to a mixed powder of 25g of TiO2 and 5g of cerium-zirconium solid solution, and ball milled at a speed of 400 rpm for 3 hours to form an active slurry with a solid content of 37.5%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 75g / L, and the carrier was obtained after drying and calcining; 10ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-dodecane was dripped to cover the catalyst surface, and the reaction was carried out at 95°C in a 0.4MPaN2 atmosphere for 2h. The catalyst was dried at 220°C under nitrogen protection and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a noble metal content of 1g / L.
[0071] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =188℃.
[0072] Example 6
[0073] 0.44g EDTA and 8.5g ammonium polyacrylate were dissolved in 40ml deionized water, and 12.5ml methanol, 48g platinum nitrate solution with a platinum content of 1% and 12g palladium nitrate solution with a palladium content of 1% were added to the solution, and the volume was adjusted to 250ml to form an impregnation solution ① with a total precious metal content of 2.4g / L; 120ml deionized water was added to a mixed powder of 25g γ-Al2O3 and 5g cerium-zirconium solid solution, and the mixture was ball-milled at a speed of 600 rpm for 0.5 hours to form an active slurry with a solid content of 20%, and then the slurry was coated on a cordierite honeycomb ceramic carrier with a coating amount of 50g / L, and the carrier was obtained after drying and calcining; 20ml of the impregnation solution ① was impregnated on 100cm 3 On the carrier, n-decane was dripped to cover the catalyst surface, and the reaction was carried out at 85°C in a 0.4MPaN2 atmosphere for 2h. The catalyst was dried at 160°C under nitrogen protection and calcined at 550°C to obtain a VOCs catalytic oxidation catalyst with a precious metal content of 0.48g / L.
[0074] The obtained catalyst was evaluated according to the above evaluation method. The evaluation results showed that 90 =195℃.
[0075] The above are only preferred feasible embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Various modifications or applications made according to the above embodiments are within the protection scope of this technical solution.
[0076] Although the specific embodiments of the present invention have been described in detail, it will be understood by those skilled in the art. According to all the teachings disclosed, various modifications and replacements can be made to those details, and these changes are all within the protection scope of the present invention. The full scope of the present invention is given by the attached claims and any equivalents thereof.
Claims
1. An oil film-wrapped in-situ reduction precious metal catalyst, characterized in that: The oil film wrapped in-situ reduction precious metal catalyst includes a carrier and nano precious metal particles loaded on the carrier, wherein the carrier is divided into a first carrier and a second carrier, the inner surface of the pores of the first carrier is coated with the second carrier, and the nano precious metal particles are distributed on the inner surface of the pores of the second carrier.
2. The oil film-wrapped in-situ reduction precious metal catalyst according to claim 1, characterized in that: The porosity of the first carrier is 20% to 95%, the positive compressive strength of the carrier is greater than 0.5 MPa, and the side compressive strength of the carrier is greater than 0.2 MPa.
3. The oil film-wrapped in-situ reduction precious metal catalyst according to claim 1, characterized in that: The first carrier is honeycomb ceramic and / or honeycomb metal.
4. The oil film-wrapped in-situ reduction precious metal catalyst according to claim 1, characterized in that: The second carrier is one of TiO2, cerium-zirconium solid solution, γ-Al2O3 and ZSM-5 molecules, or any mixture thereof.
5. The oil film-wrapped in-situ reduction precious metal catalyst according to claim 1, characterized in that: The nano noble metal includes at least one of gold, silver, ruthenium, rhodium, palladium, osmium, iridium and platinum.
6. A method for preparing the oil film-wrapped in-situ reduced precious metal catalyst as claimed in any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1: mixing the second carrier powder additive and the organic additive, and ball milling to obtain a coated catalyst slurry; S2: coating the coated catalyst slurry of S1 onto the carrier, and then drying and calcining to obtain a catalyst carrier; S3: Dissolve and mix the noble metal precursor, reducing agent, buffer and stabilizer in deionized water, and impregnate them onto the catalyst support of S2 by equal volume impregnation method, so that the impregnation liquid completely enters the micropores of the support, and then drip the coating agent to cover the surface of the support; S4: placing the impregnated support obtained in S3 in a N2 atmosphere for reaction; S5: slowly release N2 under the N2 atmosphere of S4 and dry; S6: The dried carrier is placed in a muffle furnace for calcination to obtain an oil film-coated in-situ reduced precious metal catalyst.
7. The preparation method according to claim 6, characterized in that: The encapsulating agent is an alkane oily encapsulating agent with a boiling point range of 120 to 290° C. or a water-insoluble organic substance within this boiling point range.
8. The preparation method according to claim 7, characterized in that: The encapsulating agent is n-decane, n-octane, n-dodecane or n-hexadecane.
9. The preparation method according to claim 6, characterized in that: The organic auxiliary agent is one of alcohols, aldehydes, organic acids and sodium borohydride.
10. The preparation method according to claim 6, characterized in that: The reducing agent is methanol or ethylene glycol; And / or, the stabilizer is polyvinyl pyrrolidone, polyethylene glycol or F123.
11. The preparation method according to claim 6, characterized in that: The buffer is a weak organic acid-organic acid salt system with a pH of 3-7.
12. The preparation method according to claim 11, characterized in that: The buffer is citric acid-citrate, EDTA or polyacrylic acid-polyacrylic acid.
13. The preparation method according to claim 6, characterized in that: In the step S1, the ball milling time is 0.1 to 30 hours.
14. The preparation method according to claim 6, characterized in that: In step S4, the pressure of the N2 atmosphere is 0.18MPA-0.65MPa, the volume percentage of O2 is less than 1%, the reaction time is 2-4h, and the reaction temperature is 80-95°C.
15. The preparation method according to claim 6, characterized in that: In step S5, the drying is two-end drying, the first stage drying temperature is 120°C to 300°C, and the second stage drying temperature is 300°C.
16. The preparation method according to claim 6, characterized in that: In step S6, the baking temperature is 500-600° C., and the baking time is 2-4 hours.
17. Use of the oil film coated in-situ reduction precious metal catalyst as described in claims 1 to 5 or the oil film coated in-situ reduction precious metal catalyst prepared by the preparation method according to any one of claims 6 to 16 in catalytic oxidation treatment of volatile organic compounds.
Citation Information
Patent Citations
Process for producing metal film, primer composition, metal film and use of the metal film
CN101796217A
Honeycomb catalyst for acrylonitrile device waste gas purification and preparation method thereof
CN102773120A
Soybean oil coated nano-iron slurry groundwater pollution remediation reagent and preparation method thereof
CN104773766A
Automobile exhaust gas treatment catalyst and preparation method thereof
CN109174077A
Preparation method of low noble metal diesel vehicle oxidization catalyst and catalyst prepared by using same
CN109225210A