Catalytic material for activating molecular oxygen to degrade organic pollutants as well as preparation method and application of catalytic material

Through the preparation of MoBSx catalytic material, NaBH4 and MoS2 are calcined and processed under an inert atmosphere to form a catalyst with S defects, which solves the problem of poor stability of molecular oxygen activators and achieves efficient degradation of organic pollutants in a mild environment and The stability of the catalyst is suitable for recycling.

CN119056467APending Publication Date: 2024-12-03NANJING UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410944553.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing molecular oxygen activation catalysts have poor stability under mild conditions and are difficult to achieve efficient recycling.

Method used

MoBSx catalytic material is used, which is calcined in an inert atmosphere by NaBH4 and MoS2 and treated in dilute hydrochloric acid to form a polymerized form with a large number of S defects, and an electron transfer channel from organic pollutants to O2 is constructed, and O2 is spontaneously activated to generate ROS.

Benefits of technology

Without increasing oxidant and energy consumption, it effectively degrades organic pollutants, maintains long-term catalytic activity, and is suitable for recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056467A_ABST
    Figure CN119056467A_ABST
Patent Text Reader

Abstract

The invention provides a catalytic material for activating molecular oxygen to degrade organic pollutants, and belongs to the technical field of water treatment.The structural formula of the catalytic material is MoBSx, and in the catalytic material, the atomic percent of B is 10.83%, the atomic percent of Mo is 35.5%, and the atomic percent of S is 53.67%; the catalytic material is in a polymerization form and has a large number of S defects, and the specific surface area is 4.3737 m < 2 > / g; the XRD spectrum of the catalytic material is shown in figure 3. The catalytic material constructs an electron transfer channel from organic pollutants to O2, O2 can be effectively activated to generate ROS, then various organic pollutants are degraded, and the catalytic material is good in stability and beneficial to recycling. The invention further provides a preparation method and application of the catalytic material for activating the molecular oxygen to degrade the organic pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and particularly relates to a catalytic material for activating molecular oxygen to degrade organic pollutants, a preparation method and application thereof. Background Art

[0002] Molecular oxygen (O2) is widely present in the environment and is considered to be one of the most environmentally friendly and cost-effective oxidants. However, due to the spin-forbidden reaction, the direct oxidation and degradation of organic pollutants by O2 under mild conditions is difficult. Although sufficient external energy input through photocatalysis, electrocatalysis, piezoelectricity or sonolysis can promote the activation of O2 to reactive oxygen, the high energy consumption and complex operation process limit their widespread application. With the introduction of low-carbon strategies, the spontaneous generation of ROS by O2 activation under mild environmental conditions is considered to be an environmentally friendly and economical advanced oxidation process. The existing related patents are as follows:

[0003] Comparative Publication 1: A method for treating organic wastewater by activating molecular oxygen using a micro-nano branched zero-valent copper catalyst (Patent Publication No. CN202211047249.9). This patent uses a micro-nano branched zero-valent copper catalyst to activate O2 to treat organic wastewater containing metronidazole. This material has excellent ability to activate O2 to degrade organic pollutants, which is 60.13% higher than commercial micron-grade copper powder. However, the metal is easily lost during the catalytic process and the activity decreases, which is not conducive to recycling and pollutes the water body.

[0004] Comparative Publication 2: A method for degrading ibuprofen by activating molecular oxygen using single-atom copper coupled to red phosphorus (Patent Publication No. CN202210412344.8). This patent uses transition metal Cu and the like as the active component of the catalyst, and red phosphorus as the carrier, and disperses the active component on red phosphorus by impregnation to obtain the target catalyst. This material has excellent ability to activate O2 to produce active oxidative species, but the active metal is directly exposed and easily dissolved during the catalytic process, which reduces its activity and is not conducive to recycling.

[0005] Comparative Publication 3: A preparation method and application of a molecular oxygen activation catalyst based on surface oxygen defects (Patent Publication No. CN201810254535.X). This patent constructs oxygen defects of different contents on the surface of oxides such as TiO2, MnO2 or SiO2 through the combined action of high-temperature calcination and reduction aids, and uses the formed carbon layer to stabilize and protect these oxygen defects. The obtained C@MOx material can directly react with dissolved oxygen in water to produce active oxygen species. However, the process of O2 adsorbed and reduced at the defects can easily lead to defect annihilation and thus reduce the activity of the catalytic material.

[0006] Therefore, it is of great value to develop heterogeneous Fenton catalytic materials with fast mass transfer, high activity, and multiple recycling capabilities based on constructing the electron transfer pathway from organic pollutants to O2 to generate ROS. Summary of the invention

[0007] In order to solve the problem of poor stability of existing molecular oxygen activation catalysts, the present invention provides a catalytic material for activating molecular oxygen to degrade organic pollutants. The catalytic material constructs an electron transfer channel from organic pollutants to O2, can effectively activate O2 to produce ROS, and then degrade various organic pollutants. The catalytic material has good stability and is conducive to recycling.

[0008] The invention also provides a preparation method and application of a catalytic material for activating molecular oxygen to degrade organic pollutants.

[0009] The present invention is achieved through the following technical solutions:

[0010] The present invention provides a catalytic material for activating molecular oxygen to degrade organic pollutants. The structural formula of the catalytic material is MoBSx. The atomic percentage of B in the catalytic material is 10.83%, the atomic percentage of Mo is 35.5%, and the atomic percentage of S is 53.67%.

[0011] The catalytic material is in a polymerized form, has a large number of S defects, and has a specific surface area of ​​4.3737 m 2 / g;

[0012] The XRD spectrum of the catalytic material is as follows Figure 3 shown.

[0013] In the MoBSx, 0<x<2.

[0014] Based on the same inventive concept, the present invention provides a method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants, the preparation method comprising:

[0015] Mixing NaBH4 and MoS2 and grinding them to obtain a mixture;

[0016] calcining the mixture under an inert atmosphere to obtain a black powder;

[0017] The black powder is placed in dilute hydrochloric acid, stirred for a certain period of time, and solid-liquid separation is performed to obtain black particles;

[0018] The black particles are washed, dried and ground to obtain the catalytic material MoBSx.

[0019] Preferably, the mixing of NaBH4 and MoS2 and grinding to obtain a mixture specifically comprises:

[0020] NaBH4 and MoS2 were mixed in a mass ratio of 0.5:1 and ground at 4±1°C to obtain a mixture with a particle size of 1 to 2 μm.

[0021] Preferably, calcining the mixture under an inert atmosphere to obtain a black powder specifically comprises:

[0022] The mixture was calcined under an inert atmosphere at a calcination temperature of 500±5° C., a heating rate of 4° C. / min, and a calcination time of 2±0.1 h to obtain a black powder.

[0023] Preferably, the black powder is placed in dilute hydrochloric acid, stirred for a certain period of time, and solid-liquid separation is performed to obtain black particles, which specifically includes:

[0024] The black powder was placed in dilute hydrochloric acid with a concentration of 1 mmol / L, stirred for reaction for 10±1 h, and solid-liquid separation was performed to obtain black particles.

[0025] Preferably, the black particles are washed, dried and ground to obtain the catalytic material MoBSx, which specifically comprises:

[0026] The black particles were washed several times with ethanol and deionized water respectively, and the obtained product was vacuum dried at 60±5° C. for 6±1 h. The dried product was ground to obtain a catalytic material MoBSx with a particle size of 1 to 2 μm.

[0027] Based on the same inventive concept, the present invention provides a catalytic material for activating molecular oxygen to degrade organic pollutants. The catalytic material is prepared by the above-mentioned method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants.

[0028] Based on the same inventive concept, the present invention provides an application of a catalytic material for activating molecular oxygen to degrade organic pollutants in activating molecular oxygen to generate ROS to degrade organic pollutants.

[0029] Preferably, the organic pollutants include rhodamine B and enrofloxacin.

[0030] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0031] 1. The present invention discloses a catalytic material for activating molecular oxygen to degrade organic pollutants. The catalytic material is a MoSx catalytic material doped with B and containing a large number of S defects (SVs), and its structural formula is MoBSx. Under the synergistic effect of B and SVs, the enhancement of polarization difference forms a strong interface micro-electric field on the surface of MoBSx, thereby improving the utilization efficiency of electrons in organic pollutants and promoting the transfer of electrons from organic pollutants to O2, thereby spontaneously activating O2 into ROS without increasing oxidants and energy consumption, thereby achieving oxidative decomposition of organic matter. Organic pollutants and O2 tend to be adsorbed on B and SVs, respectively, which ensures the success of the above-mentioned electron transfer pathway, so that the defects on MoBSx can maintain long-term catalytic activity.

[0032] 2. The present invention provides a catalytic material for activating molecular oxygen to degrade organic pollutants. The catalytic material is in a polymerized form and exhibits a microporous structure. According to the nitrogen adsorption / desorption isotherm and pore size distribution results, the adsorption / desorption isotherm of the catalytic material is type III, and the specific surface area is 4.3737 m 2 / g, the catalytic material constructs a transfer path for electrons from organic pollutants to O2, can effectively activate O2 to generate ROS, and then degrade various organic pollutants. In the process of activating O2 to generate ROS, there is no conversion of high and low valence states of transition metals, thereby reducing the environmental toxicity caused by metal leaching. The catalytic material of the present invention shows stability during the catalytic reaction process, and the degradation efficiency of organic pollutants is almost not reduced after continuous reaction, which is conducive to recycling.

[0033] 3. The present invention provides a method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants. The method uses NaBH4 as a B source, mixes NaBH4 with MoS2 in an inert atmosphere and then calcines the mixture. In the process, a large number of S defects are generated. The preparation process is simple. x The coupling of S defects and B atoms helps to build an electron transfer bridge on the surface of the catalytic material, resulting in a polarized distribution of electrons, which is beneficial to the controllable electron transfer from B to S defects. The prepared catalytic material realizes the directional transfer of electrons in organic pollutants to O2 through the electron transfer bridge on the surface, and has a stable removal effect on various organic pollutants in the water body, providing a promising solution for efficient O2 activation under mild environmental conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 The scanning electron microscope image (left) and transmission electron microscope image (right) of the MoBSx described in the present invention.

[0036] Figure 2 This is the N2 adsorption-desorption curve spectrum of the MoBSx described in the present invention.

[0037] Figure 3 This is the XRD pattern of MoBSx described in the present invention.

[0038] Figure 4 This is the EPR spectrum of MoBSx described in the present invention.

[0039] Figure 5 This is the EPR signal diagram of ·OH in DMPO capture suspension.

[0040] Figure 6 Capturing O2 in Suspension by DMPO ·- EPR signal diagram.

[0041] Figure 7 For TEMP capture in suspension 1 EPR signal diagram of O2.

[0042] Figure 8 This is a graph showing the degradation effect of MoBSx with different mixing ratios of NaBH4 and MoS2 on Rhodamine B (RhB) with an initial concentration of 10 ppm.

[0043] Fig. 9 This is the degradation diagram of Rhodamine B by MoBSx.

[0044] Fig.10 This is the degradation diagram of MoBSx on enrofloxacin.

[0045] Fig.11 Degradation plot for MoBSx batches used in the present invention. DETAILED DESCRIPTION

[0046] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.

[0047] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0048] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0049] The technical principle of the present invention is as follows:

[0050] The present invention provides a method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants, comprising:

[0051] S1. NaBH4 and MoS2 are mixed and ground to obtain a mixture;

[0052] S2. The mixture is calcined under an inert atmosphere to obtain a black powder;

[0053] S3. placing the black powder in dilute hydrochloric acid, stirring the reaction for a certain period of time, and obtaining black particles by solid-liquid separation;

[0054] S4. The black particles are washed, dried and ground to obtain the catalytic material MoBSx.

[0055] Step S1 specifically includes:

[0056] NaBH4 and MoS2 were mixed in a mass ratio of 0.5:1 and ground at 4±1°C to obtain a mixture with a particle size of 1 to 2 μm.

[0057] In the present invention, the optimal synthesis mass ratio of NaBH4 to MoS2 is 0.5:1, and the grinding temperature of 4±1°C is conducive to the mixing of NaBH4 and MoS2. A temperature higher than this will cause NaBH4 to liquefy.

[0058] Step S2 specifically includes:

[0059] The mixture was calcined under an inert atmosphere at a calcination temperature of 500±5° C., a heating rate of 4° C. / min, and a calcination time of 2±0.1 h to obtain a black powder.

[0060] In the present invention, the purpose of calcining the mixture under an inert atmosphere is to promote the generation of defects and prevent the catalytic material from being oxidized during the calcination process.

[0061] Step S3 specifically includes:

[0062] The black powder was placed in dilute hydrochloric acid with a concentration of 1 mmol / L, stirred for reaction for 10±1 h, and solid-liquid separation was performed to obtain black particles.

[0063] In the present invention, the purpose of placing the black powder in a diluted hydrochloric acid with a concentration of 1 mmol / L and stirring the reaction is to remove unreacted NaBH4. The stirring reaction is carried out for 10±1h. If the time is shorter than this time range, the NaBH4 in the material may not be cleaned out, thereby affecting the catalytic performance.

[0064] Step S4 specifically includes:

[0065] The black particles were washed several times with ethanol and deionized water respectively, and the obtained product was vacuum dried at 60±5° C. for 6±1 h. The dried product was ground to obtain a catalytic material MoBSx with a particle size of 1 to 2 μm.

[0066] In the present invention, the benefit of controlling the particle size of the catalytic material MoBSx within 1 to 2 μm is to promote the effective exposure of catalytic sites on the surface of the material. A particle size below or above this range is not conducive to improving the catalytic performance of the catalytic material.

[0067] The catalytic material and preparation method for activating molecular oxygen to degrade organic pollutants in the present application will be described in detail below in combination with examples and experimental data.

[0068] Example 1

[0069] This embodiment provides a method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants, comprising the following steps:

[0070] (1) NaBH4 and commercial MoS2 (Shanghai Aladdin Biochemical Technology Co., Ltd.) were mixed at a mass ratio of 0.5:1 and ground in an agate mortar at 4°C for 20 min to obtain a mixture with a particle size of 1 to 2 μm;

[0071] (2) placing the mixture obtained in step (1) in a tube furnace and calcining at 500° C. for 2 h under a N2 atmosphere at a heating rate of 4° C. / min;

[0072] (3) placing the black powder produced after calcination in step (2) in 1 mM dilute hydrochloric acid and stirring for 10 h;

[0073] (4) washing the black powder produced in step (3) with ethanol and deionized water for 6 times respectively;

[0074] (5) drying the black powder obtained in step (4) in a vacuum oven at 60° C. for 6 h;

[0075] (6) Grind the black hard solid obtained in step (5) for 10 minutes to form a powder with a particle size of 1 to 2 μm.

[0076] The catalytic material MoBSx prepared by the above method was characterized by scanning electron microscopy and transmission electron microscopy. Figure 1 .Depend on Figure 1 It can be seen that by using NaBH4 as a B source and introducing it into commercial MoS2, the synthesized catalytic material presents a polymerized morphology of a mixed phase of 1T and 2H. (2H is a stable semiconductor phase (triangular prism), and 1T is a metastable metal phase (octahedron))

[0077] Example 2

[0078] The B-doped MoSx catalytic material (MoBSx) prepared in Example 1 and containing a large amount of SVs was tested for N2 adsorption / desorption curve and pore size distribution (test instrument: Micromer it ics ASAP 2460). The results are as follows: Figure 2 shown.

[0079] Depend on Figure 2 It can be seen that the N2 adsorption / desorption isotherm of MoBSx is type III, and the specific surface area is 4.3737m 2 / g, showing a microporous structure. ( Figure 2 The two curves in the figure are the adsorption curve and the desorption curve.

[0080] Example 3

[0081] XRD characterization was performed on the B-doped MoBSx catalytic material prepared in Example 1 and containing a large amount of SVs. The single-layer or few-layer 1T phase showed weak intensity and low crystallinity in the XRD spectrum. Figure 3 It can be seen that the lower crystallinity in the XRD pattern confirms the formation of 1T phase in the MoBSx catalytic material.

[0082] Example 4

[0083] The B-doped MoBSx catalytic material prepared in Example 1 and containing a large amount of SVs was characterized by an electron paramagnetic resonance spectrometer (EPR). Figure 4 .Depend on Figure 4 It can be seen that the EPR signal is enhanced when g = 2.00, confirming the existence of S defects in the MoBSx catalytic material.

[0084] Example 5

[0085] This example measures the generation of free radicals by the MoBSx catalytic material prepared in Example 1 when activating molecular oxygen.

[0086] Test 1:

[0087] (1) Take 100 mL of a 10 ppm enrofloxacin solution prepared with ultrapure water, then add 200 uL of 5,5-dimethyl-1-pyrroline-N-oxide (DMPO), then add 0.1 g / L of MoBSx catalytic material, and then aerate with an aeration pump to obtain a liquid sample;

[0088] (2) After 5 minutes of reaction, quickly take the liquid sample described in step (1) using a spotting capillary, and then use EPR to detect the generation of free radicals in the solution.

[0089] The results are as follows Figure 5 As shown, it can be seen that:

[0090] MoBSx catalytic materials can produce a large amount of hydroxyl radicals (·OH) when activating molecular oxygen. The generation of ·OH depends on the introduction of enrofloxacin, an organic pollutant, as an electron donor.

[0091] Test 2:

[0092] (1) Take 100 mL of 10 ppm enrofloxacin solution prepared with ultrapure water, add 10 ml of methanol solution, then add 200 uL of DMPO, and then add 0.1 g / L of MoBSx catalytic material, and then aerate with an aeration pump to obtain a liquid sample;

[0093] (2) After 5 minutes of reaction, quickly take the liquid sample described in step (1) using a spotting capillary, and then use EPR to detect the generation of free radicals in the solution.

[0094] The results are as follows Figure 6 As shown, it can be seen that:

[0095] MoBSx catalytic materials can generate a large amount of superoxide radicals (O2 ·- ), O2 ·- The generation of depends on the introduction of enrofloxacin as an electron donor.

[0096] Test 3:

[0097] (1) Take 100 mL of a 10 ppm enrofloxacin solution prepared with ultrapure water, then add 1 M 2,2,6,6-tetramethylpiperidine (TEMP), then add 0.1 g / L MoBSx catalytic material, and then aerate with an aeration pump to obtain a liquid sample;

[0098] (2) After 5 minutes of reaction, quickly take the liquid sample described in step (1) using a spotting capillary, and then use EPR to detect the generation of free radicals in the solution.

[0099] The results are as follows Figure 7 As shown, it can be seen that:

[0100] MoBSx catalytic materials can generate a large amount of singlet oxygen ( 1 O2), 1 The production of O2 depends on the introduction of organic pollutants as electron donors.

[0101] Example 6

[0102] This embodiment provides a method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants, comprising the following steps:

[0103] (1) Commercial MoS2 and NaBH4 were mixed in mass ratios of 1:0.1, 1:0.5, and 1:1, respectively, and ground in an agate mortar at 4°C for 20 min to obtain a mixture with a particle size of 1 to 2 μm;

[0104] (2) placing the mixture obtained in step (1) in a tube furnace and calcining at 500° C. for 2 h under a N2 atmosphere at a heating rate of 4° C. / min;

[0105] (3) placing the black powder produced after calcination in step (2) in 1 mM dilute hydrochloric acid and stirring for 10 h;

[0106] (4) washing the black powder produced in step (3) with ethanol and deionized water for 6 times respectively;

[0107] (5) drying the black powder obtained in step (4) in a vacuum oven at 60° C. for 6 h;

[0108] (6) Grind the black hard solid obtained in step (5) for 10 minutes to form a powder with a particle size of 1 to 2 μm.

[0109] 0.1g / L MoBSx was added to 10ppm Rhodamine B (Rhodamine B) wastewater, and the solution was aerated using an aeration pump. Samples were taken at 0min, 2min, 5min, 10min, 20min and 30min, 1mL each time, and quickly filtered with a syringe filter. The obtained water samples were detected at 552nm using an ultraviolet spectrophotometer, and the degradation efficiency of Rhodamine B in different reaction systems at different times was calculated.

[0110] The results are as follows Figure 8 As shown, it can be seen that:

[0111] The MoBSx catalytic material prepared in this example exhibited the best O2 activation ability and Rhodamine B degradation efficiency when the mixture of NaBH4 and commercial MoS2 was 0.5:1.

[0112] Example 7

[0113] This example measures the activation ability of MoBSx catalytic material (NaBH4:MoS2 is 0.5:1) for molecular oxygen:

[0114] (1) Add 0.1 g / L MoBSx to 10 ppm Rhodamine B wastewater, and use an aeration pump to aerate the solution (air or argon). Sampling is performed at 0 min, 2 min, 5 min, 10 min, 20 min, and 30 min, 1 mL each time, and the samples are quickly filtered with a syringe filter. The obtained water samples are detected at 552 nm using an ultraviolet spectrophotometer, and the degradation efficiency of Rhodamine B in different reaction systems at different times is calculated;

[0115] (2) Add 0.1 g / L MoBSx to 10 ppm enrofloxacin wastewater, and use an aeration pump to aerate the solution (air, argon or oxygen). Sampling is performed at 0 min, 1 min, 2 min, 5 min, 7 min and 10 min, 1 mL each time, and the samples are quickly filtered with a syringe filter. The water samples obtained are tested by high performance liquid chromatography, and the degradation efficiency of enrofloxacin in different reaction systems at different times is calculated.

[0116] The results are as follows Fig. 9 , 10 As shown, it can be seen that:

[0117] The degradation efficiency of MoBSx catalytic material for two organic pollutants under argon conditions is much lower than that under air conditions, and the material exhibits excellent molecular oxygen activation ability.

[0118] Example 8

[0119] This example determines the stability of the MoBSx catalytic material (NaBH4: MoS2 is 0.5:1) during the molecular oxygen activation process:

[0120] (1) 0.1 g / L MoBSx was added to 10 ppm Rhodamine B wastewater, and the solution was aerated (air) using an aeration pump. Samples were taken at 0 min, 2 min, 5 min, 10 min, 20 min and 30 min, 1 mL each time, and quickly filtered with a syringe filter. The obtained water samples were detected by an ultraviolet spectrophotometer at 552 nm, and the degradation efficiency of Rhodamine B in different reaction systems at different times was calculated.

[0121] (2) The catalytic material after the reaction in step (1) was centrifuged, washed, and then vacuum dried at 60°C; 0.1 g / L of the dried catalytic material was added to 10 ppm Rhodamine B wastewater, and the solution was aerated (air) using an aeration pump, and samples were taken at 0 min, 2 min, 5 min, 10 min, 20 min, and 30 min, 1 mL each time, and quickly filtered with a syringe filter. The obtained water sample was detected at 552 nm using an ultraviolet spectrophotometer, and the degradation efficiency of Rhodamine B in different reaction systems at different times was calculated.

[0122] (3) The catalytic material after the reaction in step (2) is centrifuged, washed, and then vacuum dried at 60° C.; 0.1 g / L of the dried catalytic material is taken and added to 10 ppm rhodamine B wastewater, and the remaining operations are the same as the corresponding parts of step (2).

[0123] (4) The catalytic material after the reaction in step (3) is centrifuged, washed, and then vacuum dried at 60° C. 0.1 g / L of the dried catalytic material is taken and added to 10 ppm rhodamine B wastewater. The remaining operations are the same as the corresponding parts of step (2).

[0124] (5) The catalytic material after the reaction in step (4) is centrifuged, washed, and then vacuum dried at 60° C. 0.1 g / L of the dried catalytic material is taken and added to 10 ppm rhodamine B wastewater. The remaining operations are the same as the corresponding parts of step (2).

[0125] The results are as follows Fig.11 As shown, it can be seen that:

[0126] In the process of activating molecular oxygen to degrade organic pollutants, the degradation efficiency of the MoBSx catalytic material prepared by the present invention is not significantly reduced after being used five times in a row, and the material exhibits excellent stability.

[0127] In summary, the catalytic material MoBSx prepared by the present invention constructs an electron transfer channel from organic pollutants to O2, can effectively activate O2 to produce ROS, and then degrade various organic pollutants, and the catalytic material has good stability and is conducive to recycling. The present invention demonstrates the potential of the coupling of SVs and doped B atoms in inducing organic pollutants to act as electron donors and thus promote the activation of O2, providing a promising solution for efficient O2 activation under mild environmental conditions.

[0128] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.

[0129] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0130] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A catalytic material for activating molecular oxygen to degrade organic pollutants, characterized in that: The structural formula of the catalytic material is MoBSx, and the atomic percentage of B in the catalytic material is 10.83%, the atomic percentage of Mo is 35.5%, and the atomic percentage of S is 53.67%; The catalytic material is in a polymerized form, has a large number of S defects, and has a specific surface area of ​​4.3737 m 2 / g; The XRD spectrum of the catalytic material is shown in FIG3 .

2. A method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants, characterized in that: The preparation method comprises: Mixing NaBH4 and MoS2 and grinding them to obtain a mixture; calcining the mixture under an inert atmosphere to obtain a black powder; The black powder is placed in dilute hydrochloric acid, stirred for a certain period of time, and solid-liquid separation is performed to obtain black particles; The black particles are washed, dried and ground to obtain the catalytic material MoBSx.

3. The method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants according to claim 2, characterized in that: The mixing of NaBH4 and MoS2 and grinding to obtain a mixture specifically comprises: NaBH4 and MoS2 were mixed in a mass ratio of 0.5:1 and ground at 4±1°C to obtain a mixture with a particle size of 1 to 2 μm.

4. The method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants according to claim 2, characterized in that: The step of calcining the mixture under an inert atmosphere to obtain a black powder specifically comprises: The mixture was calcined under an inert atmosphere at a calcination temperature of 500±5° C., a heating rate of 4° C. / min, and a calcination time of 2±0.1 h to obtain a black powder.

5. The method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants according to claim 2, characterized in that: The black powder is placed in dilute hydrochloric acid, stirred for a certain period of time, and solid-liquid separation is performed to obtain black particles, which specifically includes: The black powder is placed in dilute hydrochloric acid with a concentration of 1 mmol / L, and the mixture is stirred for reaction for 10±1 h. Black particles are obtained by solid-liquid separation.

6. The method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants according to claim 2, characterized in that: The black particles are washed, dried and ground to obtain the catalytic material MoBSx, which specifically comprises: The black particles were washed several times with ethanol and deionized water respectively, and the obtained product was vacuum dried at 60±5° C. for 6±1 h. The dried product was ground to obtain a catalytic material MoBSx with a particle size of 1 to 2 μm.

7. A catalytic material for activating molecular oxygen to degrade organic pollutants, characterized in that: The catalytic material is prepared by the method for preparing a catalytic material for activating molecular oxygen to degrade organic pollutants according to any one of claims 2 to 6.

8. Use of the catalytic material for activating molecular oxygen to degrade organic pollutants as claimed in claim 1 or 7 in activating molecular oxygen to generate ROS to degrade organic pollutants.

9. The use according to claim 8, characterized in that: The organic pollutants include rhodamine B and enrofloxacin.