Preparation method of acidic hydrodeoxygenation catalyst, obtained product and application of product in preparation of biofuel by catalyzing biolipid
Through the preparation of acidic Mo2C/modified biochar catalyst, the problems of large hydrogen consumption and short catalyst life in the hydrodeoxygenation process of bio-oil are solved, efficient and low-cost biofuel production is achieved, and the application prospects of catalysts are improved.
Patent Information
- Application Number
- CN202411173013.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing hydrodeoxygenation catalysts of biooils have problems such as large hydrogen consumption, coking and short catalyst life under high pressure and high temperature conditions, and the cost of precious metal catalysts is high, which affects its application prospects.
Acid Mo2C/modified biochar catalyst is used to acidify biochar by concentrated nitric acid and load ammonium molybdate, combined with carbon-heat hydrogen reduction reaction, which reduces costs and improves catalytic activity.
The high conversion rate of bio-oil and the production of high-quality biofuels are achieved, which reduces catalyst costs, extends the catalyst life, and avoids the safety risks of high pressure and high temperatures.
Smart Images

Figure CN119056476A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of an acidic Mo2C / modified AC hydrodeoxygenation catalyst and the obtained Mo2C / modified AC hydrodeoxygenation catalyst, and also relates to application of the catalyst in catalyzing bio-oil to prepare biofuel. Background Art
[0002] Energy is the foundation of social industry and an important driving force for social and economic development. However, today's society is facing serious problems such as fossil energy depletion and environmental pollution. Correspondingly, the scale of global renewable energy development and utilization is constantly expanding. The development of renewable energy has become the core content of many countries in promoting energy transformation and an important way to cope with climate change.
[0003] Among many renewable resources, biomass resources have attracted extensive attention due to their wide sources, renewability and carbon neutrality. In the process of developing and utilizing renewable resources, the preparation of biofuels has the greatest research and development potential.
[0004] WO2019019539A1 points out that bio-oil has the potential to replace fossil fuel oil. At present, bio-oil is mainly used for boiler fuel or automotive blending oil, but has not completely replaced automotive fuel. The main reason is that bio-oil has a complex composition (including acids, alcohols, aldehydes, esters, ketones, phenols and guaiacol), high oxygen content, high viscosity (650cP at 40°C, heavy petroleum fuel oil is 180cP at 40°C), low calorific value (bio-oil is generally around 28MJ / Kg, heavy petroleum fuel oil is 40MJ / Kg), strong acidity and poor low-temperature fluidity. These factors lead to the shortcomings of bio-oil, such as poor chemical stability, low calorific value, complex composition, and corrosiveness. Therefore, bio-oil must be refined to replace fossil fuel oil.
[0005] Bio-oil upgrading methods include extraction, solvent addition, emulsification, esterification / alcoholysis, supercritical fluid (SCF), hydrotreating, catalytic cracking and steam reforming. Hydrotreating is carried out at moderate temperatures (300-450°C) and high pressure (up to 20MPa) of hydrogen source and has been proven to be an effective bio-oil upgrading method for removing heteroatoms (O, N and S). During the hydrotreating of bio-crude oil, O is removed in the form of water, and N and S are removed in the form of NH3 and H2S, respectively. Most bio-oils do not contain significant concentrations of N and S, so the hydrotreating of bio-oil is essentially hydrodeoxygenation (HDO).
[0006] The catalysts for HDO can be divided into sulfides, oxides, precious metals, phosphides and carbides according to the active components. Sulfide catalysts play an important role in the oil refining industry and have been widely used to remove S and N elements from crude oil. Usually, Mo is used as the main active metal and Ni or Co is used as a promoter, supported on SiO2 or Al2O3. For example, the phenol conversion rate of Ni-Mo sulfided catalyst is 96.2% higher than that of Mo sulfided catalyst, which is due to the addition of Ni promoter to promote the hydrogen activation process of Mo-s. Based on the H2-temperature programmed desorption (TPD) results, the binary Ni-Mo catalyst is more active than the single Mo or Ni sulfided catalyst, which is due to the promotion effect of Ni in the Mo catalyst. In order to reduce the deactivation of the catalyst in the HDO process, a certain amount of sulfiding agent such as hydrogen sulfide is added to the reactor of low-sulfur bio-oil feedstock, which may increase the sulfur content in the upgraded finished oil. The addition of additional sulfur sources may also lead to catalyst poisoning in the subsequent process and SOx emissions during combustion. To solve this problem, oxides of Mo, Ni, and W have been tested and shown to exhibit strong catalytic activity in the HDO of bio-oil and its model compounds. Precious metal catalysts such as Pt, Pd, Rh, and Ru show high catalytic activity in the HDO treatment of bio-oil, but the price of precious metals is high, which greatly increases the cost of use.
[0007] Catalysts such as metal phosphides, nitrides, and carbides are also widely used in HDO catalysis of bio-oil. From an economic point of view, it is more desirable to use non-precious metal catalysts for bio-oil upgrading. Metal phosphide catalysts are widely used in the oil refining industry due to their low activation energy and high catalytic activity. In recent years, they have received extensive attention in the HDO of bio-oil and its model compounds, which is mainly attributed to the presence of their acidic sites and h2 activation sites. In addition, metal carbides and nitrides show great prospects in bio-oil HDO because of their low cost and catalytic activity comparable to traditional HDO catalysts.
[0008] In the HDO of bio-oil, the yield and performance of the upgraded bio-oil depend on the temperature, residence time, hydrogen pressure, solvent, and catalyst type. Although catalytic HDO has broad application prospects and effectiveness in the process of bio-oil upgrading, high hydrogen consumption, coking, and short catalyst life are the main obstacles restricting its application. The most commonly used temperature range for the HDO process is 250-400 °C. Generally, temperatures above 450 °C are not conducive to the HDO upgrading of crude bio-oil due to the exothermic nature of HDO and accelerated coke formation. High-pressure hydrogen (i.e., 10-30 MPa), especially at high temperatures, is a necessary condition for the catalytic HDO process. Higher H2 pressure not only ensures good solubilization of H2 in the HDO reaction medium, but also helps to stabilize the unstable precursors (i.e., high molecular weight intermediates) derived from bio-oil, thereby delaying the formation of coke and extending the life of the catalyst. Although high H2 pressure can limit the formation of coke and promote the HDO reaction, the high pressure greatly increases the requirements for the reaction equipment and the high-pressure condition also leads to certain safety issues.
[0009] Liu Xiaoran et al. studied the preparation of Mo2C / MCM-41 and its catalytic performance in the hydrogenation of carbon dioxide, indicating that Mo2C exhibits high catalytic activity in the hydrogenation of carbon dioxide, has strong resistance to sulfur and chlorine poisoning, and has good reaction stability. Li Henan et al. studied the preparation of modified Mo2C / MCM-41 and its catalytic performance in the hydrogenation of carbon dioxide, and prepared MgO-Mo2C / MCM-41 catalyst modified by MgO, which significantly improved the catalytic activity of the hydrogenation of carbon dioxide.
[0010] Ochoa et al studied the hydrothermal enhancement of the synthesis of highly selective Mo2C catalysts for complete deoxygenation of guaiacol in the hydrodeoxygenation (HDO) reaction. The hydrothermal impregnation resulted in the highest surface atomic Mo / C ratio. The HDO of guaiacol at 300 °C and 34 barH2 gave a maximum guaiacol conversion of 97% and a maximum HDO ratio of 84%.
[0011] Xiangze Du et al. studied the efficient conversion of jatropha oil into high-quality biofuels using Ni-Mo2C / MCM-41 catalysts. During the conversion of jatropha oil (JO), the activity of the Ni-Mo2C / MCM-41 catalyst changed like a volcano as the CH4 content increased from 15% to 50%. The Ni-Mo2C(25) / MCM-41 prepared with 25% CH4 content had excellent catalytic performance, with a biofuel yield of 83.9wt% and a C15-C18 selectivity of 95.2%.
[0012] CN116651476A discloses a method for preparing a transition metal-loaded zirconium phosphate grease catalyst, wherein the active component is loaded onto a zirconium phosphate carrier and the hydrodeoxygenation single factor experiment is conducted to find that the best hydrodeoxygenation effect of the catalyst band is obtained under the conditions of reaction temperature 280-400°C, hydrogen pressure 2-6MPa, and reaction time 2-10h. The application does not use precious metal elements, so the production cost of the catalyst is low. When the zirconium-phosphorus ratio is 1, the conversion rate of methyl palmitate reaches a maximum of 97% but does not reach 100%, and some methyl palmitate does not react. Moreover, the optimal experimental condition hydrogen pressure is 6MPa. Too high a reaction pressure not only causes hydrogen waste but also has certain production safety issues. Summary of the invention
[0013] The purpose of the present invention is to provide a method for preparing an acidic hydrodeoxygenation catalyst and the resulting product. The acidic hydrodeoxygenation catalyst is Mo2C / modified biochar (AC) with certain acidity. The preparation method is simple, and transition metals are used as active ingredients and cheap bioactivated carbon is used as a carrier, which greatly reduces the cost of the catalyst. The catalyst can catalyze the conversion of bio-oil into biofuel, has a high conversion rate, and has good biofuel quality, and has a good application prospect.
[0014] In order to achieve the above object, the present invention adopts the following technical solutions:
[0015] A method for preparing an acidic hydrodeoxygenation catalyst, the method comprising the following steps:
[0016] (1) acidifying the biological activated carbon with concentrated nitric acid to obtain modified biological activated carbon;
[0017] (2) loading ammonium molybdate onto modified biological activated carbon by an impregnation method to obtain a catalyst precursor;
[0018] (3) Carbothermal hydrogen reduction reaction is carried out in a hydrogen atmosphere, the catalyst precursor is first heated to 430-470°C at a heating rate of 4-6°C / min, and then heated to 680-720°C at a heating rate of 0.5-1.5°C / min, and the reaction is carried out by heat preservation. After the reaction, the catalyst is naturally cooled to room temperature in nitrogen to obtain an acidic hydrodeoxygenation catalyst, which is Mo2C / modified bioactivated carbon with acidity.
[0019] Furthermore, in step (1), the bioactivated carbon is obtained by high-temperature carbonization of coconut skin, which refers to the mesocarp of coconut, a thick and loose brown fiber layer. The present invention selects the inexpensive and easily available waste tropical biomass coconut skin to prepare bioactivated carbon, which not only reduces the cost, but also realizes the high-value recycling of waste coconut skin.
[0020] In a specific embodiment of the present invention, a method for preparing bioactivated carbon (AC) is provided, the operation of which comprises: heating coconut shell powder to 580-620°C at a rate of 18-22°C / min under gas protection, and keeping the temperature for 20-30 minutes to obtain bioactivated carbon.
[0021] Furthermore, in step (1), the present invention acidifies the bio-activated carbon, and the acidified coconut shell bio-activated carbon carrier has a certain weak acidity, and there is Acid and Lewis acid, the acidity is enhanced after loading Mo2C, and the Lewis acid has the largest increase. The appropriate acid site is conducive to promoting the activation of CO bonds in the catalyst hydrodeoxygenation reaction and promoting the deoxygenation reaction. Preferably, the bioactivated carbon and concentrated nitric acid are mixed and stirred for 24-26 hours for acidification, and then washed and dried to obtain modified bioactivated carbon. The concentration of concentrated nitric acid is greater than or equal to 6mol / L, such as 6mol / L, 7mol / L, 8mol / L, 9mol / L, 10mol / L, 11mol / L, 12mol / L, etc., or any range therebetween. The dosage relationship of bioactivated carbon and concentrated nitric acid can be 1g:40-60ml, such as 1g:40ml, 1g:50ml, 1g:60ml.
[0022] Further, in step (2), the required amount of ammonium molybdate is loaded onto the modified bio-activated carbon by an impregnation method. The amount of ammonium molybdate is determined according to the final loading amount of Mo2C on the modified bio-activated carbon, and the loading amount of Mo2C on the modified bio-activated carbon is generally 10-25wt%, such as 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%. The loading amount is calculated as catalyst loading amount = active component mass / (carrier mass + active component mass). The amount of ammonium molybdate is calculated, and then the ammonium molybdate is prepared into a solution of suitable concentration, and the modified bio-activated carbon is impregnated into the solution, and the solution is dried after being completely absorbed to obtain a catalyst precursor.
[0023] Furthermore, in order to improve the loading efficiency of ammonium molybdate, the mixture of the ammonium molybdate solution and the modified biological activated carbon can be assisted by at least one of heating and stirring.
[0024] Furthermore, in step (3), the catalyst precursor is placed in a tubular furnace, and the temperature is first raised to 430-470°C at a heating rate of 4-6°C / min in a hydrogen reducing atmosphere, and then raised to 680-720°C at a heating rate of 0.5-1.5°C / min, and then kept at this temperature for 2-3 hours to perform a carbon thermal hydrogen reduction reaction. After the reaction is completed, the introduction of hydrogen is stopped, and nitrogen is introduced for passivation until it naturally drops to room temperature to obtain an acidic Mo2C / modified biological activated carbon hydrodeoxygenation catalyst.
[0025] The present invention also provides an acidic hydrodeoxygenation catalyst (acidic Mo2C / modified bioactivated carbon) prepared according to the above method and the use of the catalyst in catalyzing the conversion of bio-oil into biofuel. The catalyst can catalyze the hydrodeoxygenation reaction of bio-oil, reduce the oxygen content in the bio-oil, and convert the bio-oil into alkane biofuel.
[0026] The present invention also provides a method for preparing biofuel, which uses bio-oil as a raw material and obtains the biofuel by a hydrodeoxygenation reaction under the catalysis of the above-mentioned acidic hydrodeoxygenation catalyst.
[0027] Furthermore, the bio-oil includes jatropha oil and the like.
[0028] Furthermore, the bio-oil, solvent and catalyst are mixed, and then hydrogen is introduced to carry out a hydrodeoxygenation reaction.
[0029] Furthermore, the solvent may be n-hexane or the like. The solvent provides a medium environment, and its dosage can be adjusted as needed. For example, the mass ratio of bio-oil to solvent is 1:8-15.
[0030] Further, the amount of the catalyst is 5-20% of the mass of the bio-oil, such as 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%. Within this range, as the catalyst content increases, the content of oxygenated compounds and olefins in the obtained product shows a downward trend, and the content of alkanes shows an upward trend. When the catalyst content is 20%, the content of oxygenated compounds and olefins reaches the lowest value, and the content of alkanes reaches the highest value.
[0031] Further, the hydrogen pressure is 0.5-4Mpa, such as 0.5Mpa, 1Mpa, 2Mpa, 3Mpa, 4Mpa. Within this range, as the hydrogen pressure increases, the oxygen-containing compound and olefin content of the obtained product show a downward trend, but the downward trend is not obvious, and the alkane content shows an upward trend.
[0032] Further, the reaction temperature is 280-360° C., for example, 280° C., 290° C., 300° C., 310° C., 320° C., 330° C., 340° C., 350° C., 360° C. Within this range, as the reaction temperature increases, the contents of oxygenated compounds and olefins in the obtained product show a downward trend, and the content of alkanes shows an upward trend.
[0033] The reaction time is generally 3-6 h, for example 3 h, 4 h, 5 h, 6 h, preferably 5 h.
[0034] Furthermore, when the bio-oil raw material is jatropha oil, the conversion rate of jatropha oil is 100%, and the obtained product has a high content of alkane components and is mainly biodiesel, followed by biogasoline and biojet fuel components.
[0035] The present invention utilizes waste tropical biomass coconut shells to crack and prepare bioactivated carbon and then performs acid modification. The modified bioactivated carbon and ammonium molybdate solution are impregnated and carbon thermal hydrogen reduced to obtain a new hydrodeoxygenation catalyst acidic Mo2C / modified AC. Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The raw materials of the catalyst of the present invention are biological activated carbon and ammonium molybdate prepared from waste coconut shells, and the raw materials are simple and easy to obtain.
[0037] 2. The acidic catalyst Mo2C / modified AC of the present invention uses Mo2C as the active component, which has a price advantage over precious metal elements and does not contain environmentally polluting elements such as S. The catalyst of the present invention uses cheap biological activated carbon to provide a carbon source to prepare Mo2C. The biological activated carbon kills two birds with one stone, namely, providing a carbon source for the generation of Mo2C and providing a large specific surface area as a carrier for the dispersion of active components, which greatly reduces the cost of the catalyst.
[0038] 3. The present invention uses acid-modified coconut shell bioactivated carbon as a carrier. The acid-modification increases the acid sites of the carrier, which is beneficial to promoting the activation of CO bonds in the catalyst hydrodeoxygenation reaction and promoting the deoxygenation reaction.
[0039] 4. The catalyst of the present invention has a good hydrogenation effect, and its hydrogenation deoxygenation performance is comparable to that of precious metals. The catalytic conversion rate of jatropha oil can reach nearly 100%, and the oxygen-containing compounds in the obtained biofuel can be reduced to a minimum of 0.49%, and the olefin content can be reduced to a minimum of 0.32%, with a high deoxygenation rate.
[0040] 5. The selectivity of alkanes in the biofuel product of the present invention can be as high as 99%, and the alkanes are mainly octadecane and heptadecane, which ensures the integrity of the alkane carbon chain and reduces the occurrence of cracking reactions. Taking jatropha oil as an example, the biofuel converted from jatropha oil contains up to 99.18wt% alkanes, of which the content of the generated oil C15-C18 biodiesel component is as high as 94.3wt%, and the content of C7-C14 biogasoline and biojet fuel components is as high as 4.8wt%. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The XRD characterization results of the obtained acidic Mo2C / modified AC catalyst.
[0042] Figure 2 The SEM characterization results of the obtained acidic Mo2C / modified AC catalyst.
[0043] Figure 3 This is the TEM effect diagram of the obtained acidic Mo2C / modified AC catalyst.
[0044] Figure 4 Mo3d spectrum of Mo2C catalyst based on XPS analysis of acidic Mo2C / modified AC catalyst.
[0045] Figure 5 Pyridine infrared spectra of modified bioactivated carbon support and acidic Mo2C / modified AC catalyst. DETAILED DESCRIPTION
[0046] The present invention will be further described in detail below in conjunction with specific examples to make the advantages of the present invention more obvious. It should be understood that the contents thereof are only used for illustration and are by no means intended to limit the scope of protection of the present invention. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0047] Example 1
[0048] 1. Use a grinder to crush the dried coconut skin, then pass it through a 60-mesh sieve to obtain coconut skin powder. Spread the coconut skin powder in a crucible and push it into the middle of a microwave pyrolysis furnace. Keep the nitrogen flow rate at 100 mL / min, heat it to 600°C at a rate of 20°C / min, and react for 20 minutes to obtain biological activated carbon (AC) powder.
[0049] 2. Add 4 g of bioactivated carbon powder and 200 mL of HNO3 solution (6 mol / L) into a beaker, stir at room temperature for 24 h, filter after stirring, rinse with plenty of water until the pH value is 7, and then dry at 100 ° C overnight to obtain a purified modified bioactivated carbon carrier.
[0050] 3. Add 1 g of purified modified biological activated carbon, 0.325 g of ammonium molybdate tetrahydrate and 15 mL of deionized water into a beaker, stir magnetically in a water bath at 80 °C for 3 h, and dry at 120 °C overnight after the solution is completely absorbed to obtain a catalyst precursor.
[0051] 4. Calcinate the catalyst precursor in a hydrogen atmosphere: first increase the temperature from room temperature to 450°C at a rate of 5°C min -1 ; Then slowly increase the temperature to 700℃, the heating rate is 1℃min -1 ; Carbohydride reduction reaction was carried out in situ at 700°C in hydrogen atmosphere for 2 hours. After the calcination reaction, the hydrogen was turned off, nitrogen was introduced and cooled to room temperature to obtain an acidic Mo2C / modified AC catalyst, in which the loading amount of Mo2C in the catalyst was 15%.
[0052] Figure 1 Figure 2 is the XRD characterization result of the obtained acidic Mo2C / modified AC catalyst. Combined with the standard spectrum (PDF#71-0242), it shows that the characteristic peaks formed by the molybdenum carbide catalyst are obvious, and molybdenum carbide crystals are formed at 34.3°, 38.0°, 39.4°, 52.1°61.7°, 69.4°, and 74.7°, respectively.
[0053] Figure 2 and Figure 3 The SEM and TEM images of the obtained acidic Mo2C / modified AC catalyst are respectively. It can be seen from the figure that the active components of the catalyst are evenly distributed on the modified biological activated carbon carrier, and no obvious agglomeration occurs.
[0054] Figure 4 According to the Mo3d spectrum of acidic Mo2C / modified AC XPS analysis, there are 228.36eV, 229.78eV, 230.38eV, 231.28eV, 232.98eV, and 236.13eV peaks in the spectrum, of which 228.36eV belongs to Mo 2+ 3d 5 / 2 orbital, 230.38eV, 231.28eV belong to Mo δ+ 3d 5 / 2 (2<δ<4) orbital, 229.78eV belongs to Mo 4+ 3d 5 / 2 orbital, 232.98eV, 236.13eV belong to Mo 6+ 3d 3 / 2 Orbit. δ+ It can be attributed to Mo-C species and is related to the formation of molybdenum carbide. 2+ and Mo δ+ As the main catalytic active site, Mo 4+ and Mo6+ This may be related to the oxidation of O2 into MoO2 and MoO3 when the catalyst is exposed to air.
[0055] Figure 5 The pyridine infrared spectra of the modified biological activated carbon carrier and the acidic Mo2C / modified AC catalyst are shown in the figure. -1 、1488cm -1 、1541cm -1 、1629cm -1 、1635cm -1 There are characteristic peaks, including 1445cm -1 It is the characteristic peak of Lewis acid, proving that both the modified AC and Mo2C / modified AC contain Lewis acid, 1488cm -1 The characteristic peak is Acid and Lewis acid work together to achieve, 1541cm -1 、1629cm -1 、1635cm -1 yes The results are achieved by acid action, which proves that modified AC and acidic Mo2C / modified AC contain Acid. The quantitative table of catalyst acidity in Table 1 below was obtained by analyzing the data with pyridine infrared detection. The table shows that at 350°C, both modified AC and acidic Mo2C / modified AC are 0, which proves that neither the carbon carrier nor the catalyst has strong acid sites. At 200°C, both modified AC and acidic Mo2C / modified AC have data, but the strong acid spectrum shows 0. Combined with the pyridine infrared spectrum, it can be determined that the carbon carrier and acidic Mo2C / modified AC contain relatively weak B acid and L acid. After undergoing acidic activation, part of the surface of biochar may be oxidized by acid. When combined with H, active H sites are formed. The active H sites easily release H ions to form B acid. Therefore, the activated biological activated carbon may contain a certain amount of B acid and L acid. Appropriate acid sites are conducive to promoting the activation of CO bonds in the catalyst hydrodeoxygenation reaction and promoting the deoxygenation reaction.
[0056] Table 1 Quantitative table of acidity of catalysts and supports at 200°C and 350°C
[0057]
[0058] Example 2
[0059] In a 100 ml intermittent reactor, 1 g of the reaction substrate jatropha oil, 10 g of n-hexane, and 0.1 g of the acidic Mo2C / modified AC catalyst of Example 1 were added, hydrogen was introduced to maintain the pressure in the reactor at 2 MPa, and then the temperature was raised to 280° C. for reaction for 4 h to obtain a bioalkane fuel. After the reaction was completed, the temperature was lowered to room temperature, the pressure was vented, and the reaction product was analyzed using a gas chromatography-mass spectrometry (GC-MS).
[0060] Example 3
[0061] The bioalkane fuel was prepared according to the method of Example 2, except that the reaction temperature was 330°C.
[0062] Example 4
[0063] The bioalkane fuel was prepared according to the method of Example 2, except that the reaction temperature was 340°C.
[0064] Example 5
[0065] The bioalkane fuel was prepared according to the method of Example 2, except that the reaction temperature was 350°C.
[0066] Example 6
[0067] In a 100 ml intermittent reactor, 1 g of the reaction substrate jatropha oil, 10 g of n-hexane, and 0.1 g of the acidic Mo2C / modified AC catalyst of Example 1 were added, hydrogen was introduced to maintain the pressure in the reactor at 2 MPa, and then the temperature was raised to 360° C. for reaction for 4 h to obtain a bioalkane fuel. After the reaction was completed, the reaction mixture was cooled to room temperature, the pressure was vented, and the reaction product was analyzed using a gas chromatography-mass spectrometry (GC-MS).
[0068] Example 7
[0069] The bioalkane fuel was prepared according to the method of Example 6, except that hydrogen was introduced to maintain the pressure in the reactor at 0.5 MPa.
[0070] Example 8
[0071] The bioalkane fuel was prepared according to the method of Example 6, except that hydrogen was introduced to maintain the pressure in the reactor at 1 MPa.
[0072] Example 9
[0073] The bioalkane fuel was prepared according to the method of Example 6, except that hydrogen was introduced to maintain the pressure in the reactor at 3 MPa.
[0074] Example 10
[0075] The bioalkane fuel was prepared according to the method of Example 6, except that hydrogen was introduced to maintain the pressure in the reactor at 4 MPa.
[0076] Embodiment 11
[0077] The bioalkane fuel was prepared according to the method of Example 6, except that the reaction time was 3 h.
[0078] Example 12
[0079] In a 100 ml batch reactor, 1 g of the reaction substrate jatropha oil, 10 g of n-hexane, and 0.1 g of the acidic Mo2C / modified AC catalyst of Example 1 were added, hydrogen was introduced to maintain the pressure in the reactor at 2 MPa, and then the temperature was raised to 360° C. for reaction for 5 h to obtain bioalkane fuel. After the reaction was completed, the temperature was lowered to room temperature, the pressure was vented, and the reaction product was analyzed using a gas chromatography-mass spectrometry (GC-MS) instrument.
[0080] Example 13
[0081] The bioalkane fuel was prepared according to the method of Example 6, except that the reaction time was 6 h.
[0082] Embodiment 14
[0083] Bioalkane fuel was prepared according to the method of Example 12, except that the amount of catalyst used was 0.05 g.
[0084] Embodiment 15
[0085] Bioalkane fuel was prepared according to the method of Example 12, except that the amount of catalyst used was 0.15 g.
[0086] Example 16
[0087] Bioalkane fuel was prepared according to the method of Example 12, except that the amount of catalyst used was 0.2 g.
[0088] Comparative Example 1
[0089] A hydrodeoxygenation catalyst was prepared according to the method of Example 1, except that step 2 was omitted and the bioactivated carbon was not acid-modified to obtain a Mo2C / AC catalyst.
[0090] Bioalkane fuel was prepared according to the method of Example 12, except that the catalyst used was the Mo2C / AC catalyst prepared in this comparative example.
[0091] Comparative Example 2
[0092] The hydrodeoxygenation catalyst was prepared according to the method of Example 1, except that in step 4, the catalyst precursor was calcined in a hydrogen atmosphere from room temperature to 700°C at a heating rate of 5°C min -1 After the calcination reaction, the hydrogen was turned off and nitrogen was introduced to cool to room temperature to obtain the Mo2C / modified AC catalyst.
[0093] Bioalkane fuel was prepared according to the method of Example 12, except that the catalyst used was the Mo2C / modified AC catalyst prepared in this comparative example.
[0094] Comparative Example 3
[0095] 1 g of MCM-41, 0.325 g of ammonium molybdate tetrahydrate and 15 mL of deionized water were added to a beaker, and the mixture was magnetically stirred in a water bath at 80° C. for 3 h. After the solution was completely absorbed, the mixture was dried at 120° C. overnight to obtain a catalyst precursor.
[0096] The catalyst precursor was calcined in a CH4 atmosphere: first, the temperature was raised from room temperature to 450 °C at a rate of 5 °C min -1 ; Then slowly increase the temperature to 700℃, the heating rate is 1℃min -1 ; The reaction was carried out at 700°C in a CH4 atmosphere for 2 hours. After the calcination reaction was completed, the mixture was naturally cooled to room temperature in a nitrogen atmosphere to obtain a Mo2C / MCM-41 catalyst.
[0097] Bioalkane fuel was prepared according to the method of Example 12, except that the catalyst used was the Mo2C / MCM-41 catalyst prepared in this comparative example.
[0098] Comparative Example 4
[0099] Weigh 0.325g of ammonium molybdate tetrahydrate and dissolve it in 15ml of distilled water, then drop it into 1g of melamine, ultrasonicate for 1h, and vacuum dry at 80℃ for 12h to obtain a catalyst precursor. Place the catalyst precursor in a tubular furnace and program the temperature under 150mL / min nitrogen conditions, from room temperature to 700℃ at a heating rate of 3℃ / min, and keep it for 3h. After the furnace temperature drops to room temperature, switch the gas to 1vol% O2 / N2 and passivate for 6h to obtain a MoC / CN catalyst.
[0100] Bioalkane fuel was prepared according to the method of Example 12, except that the catalyst used was the MoC / CN catalyst prepared in this comparative example.
[0101] Comparative Example 5
[0102] The bioalkane fuel was prepared according to the method of Example 12, except that no catalyst was added.
[0103] The components of the bioalkane fuels obtained in each example and comparative example are shown in Table 2 below:
[0104] Table 2
[0105]
[0106]
[0107] From the comparison of Examples 2-6, it can be seen that when the reaction temperature is low at 280°C, the deoxygenation effect of the catalyst is very poor, a large amount of fatty acids do not participate in the reaction, and with the increase of the reaction temperature, the content of oxygenated compounds and olefins shows a downward trend, while the content of alkanes shows an upward trend. At a reaction temperature of 360°C, the content of oxygenated compounds reaches a minimum of 0.96%, the content of olefins reaches a minimum of 2.38%, and the content of alkanes reaches a maximum of 96.70%. Therefore, the reaction temperature is preferably 330-360°C, more preferably 360°C.
[0108] From the comparison of Examples 6, 7-10, it can be seen that in Example 7, because the hydrogen pressure is 0.5 MPa, the olefin content is as high as 20.74%, proving that a certain amount of hydrogen is required for the hydrodeoxygenation reaction. As the hydrogen pressure increases, the oxygen-containing compound and olefin content also show a downward trend, but the downward trend is no longer obvious, and the alkane content shows an upward trend. When the hydrogen pressure is 4 MPa in Example 10, the oxygen-containing compound content drops to a minimum of 0.93%, but it is not much different from the oxygen-containing compound content of 0.96% at 2 MPa in Example 6. When the hydrogen pressure is 3 MPa in Example 9, the olefin content reaches a minimum of 0.34%. Therefore, the hydrogen pressure is preferably 1-4 MPa.
[0109] From the comparison of Examples 6, 11-13, it can be seen that the shorter reaction time of 3h in Example 11 is not conducive to the hydrogenation reaction, and the olefin content reaches 6.85%. With the increase of reaction time, the oxygen-containing compound content and the olefin content tend to decrease, and reach the lowest 0.49% and 0.33% respectively in Example 12 after 5h of reaction, and the alkane content reaches the maximum 99.18%. As the reaction temperature continues to increase, the oxygen-containing compound and olefin content tend to increase when the reaction time is longer than 6h in Example 13, proving that a longer reaction time is also not conducive to the occurrence of hydrodeoxygenation reaction.
[0110] From the comparison of Example 12, Examples 14-16, and Comparative Example 5, it can be seen that when the catalyst content in Comparative Example 5 is 0g, the reaction product contains a large amount of oxygenated compounds and olefins, with contents of 38.76% and 47.15%, respectively, and the alkane content is only 11.86%, and the alkane selectivity is very low, proving that the hydrodeoxygenation reaction of bio-oils requires the participation of a certain catalyst. As the catalyst content increases, the content of oxygenated compounds and olefins shows a decreasing trend, while the alkane shows an increasing trend, and the best effect is achieved at 0.2g of the catalyst in Example 16, with oxygen content of 0.49%, olefins of 0.32%, and alkanes of 99.19%. However, the effects of Example 12 and Example 16 are comparable, and based on cost considerations, the catalyst dosage is preferably 0.1g.
[0111] From the comparison between Example 12 and Comparative Examples 1-4, it can be seen that the selection of the catalyst carrier and the preparation method of the catalyst of the present invention play an important role in improving the catalyst performance.
[0112] Analysis of the component structure of the bioalkane fuel obtained in Example 12 showed that the conversion rate of jatropha oil was 100%, wherein the content of C15-C18 biodiesel components was as high as 94.3wt%, and the content of C7-C14 biogasoline and bio-jet kerosene components was 4.8wt%. It can be seen that after the jatropha oil is hydrodeoxygenated by the catalyst of the present invention, the alkane component content in the obtained product is high and mainly biodiesel, followed by biogasoline and bio-jet kerosene components, and the yield of jatropha oil biodiesel is high.
[0113] It can be seen from the above experiments that the combination of molybdenum carbide and modified biochar carrier in the catalyst of the present invention shows a synergistic effect in the catalytic hydrodeoxygenation reaction, and the acidity of the Mo2C / modified AC catalyst helps to improve the catalytic effect of the catalyst, promote the CO bond cleavage and hydrogenation reaction of jatropha oil, so that the content of oxygen-containing compounds in the product is low, that is, the deoxygenation rate is high, the alkane content is high and the olefin content is low. The optimal reaction conditions of the catalyst of the present invention for jatropha oil are: catalyst dosage 10%, hydrogen pressure 2Mpa, reaction temperature 360°C, reaction time 5h, reaction temperature and hydrogen pressure are both low, and cost and safety are reduced.
Claims
1. A method for preparing an acidic hydrodeoxygenation catalyst, Its characteristics are The following steps are involved: (1) acidifying the biological activated carbon with concentrated nitric acid to obtain modified biological activated carbon; (2) loading ammonium molybdate onto modified biological activated carbon by an impregnation method to obtain a catalyst precursor; (3) Carbothermal hydrogen reduction reaction is carried out in a hydrogen atmosphere, the catalyst precursor is first heated to 430-470°C at a heating rate of 4-6°C / min, and then heated to 680-720°C at a heating rate of 0.5-1.5°C / min, and the reaction is carried out at a temperature preservation rate. After the reaction, the catalyst precursor is naturally cooled to room temperature in nitrogen to obtain acidic Mo 2 C / modified biological activated carbon hydrodeoxygenation catalyst.
2. The preparation method according to claim 1, Its characteristics are: In step (1), the biological activated carbon is obtained by high-temperature carbonization of coconut shells; preferably, the preparation method of the biological activated carbon is: heating the coconut shell powder to 580-620°C at a rate of 18-22°C / min under gas protection, and keeping the temperature for 20-30 minutes to obtain the biological activated carbon.
3. The preparation method according to claim 1, Its characteristics are: In step (1), the biological activated carbon and concentrated nitric acid are mixed and stirred for 24-26 hours, then washed with water and dried to obtain modified biological activated carbon; preferably, the ratio of biological activated carbon to concentrated nitric acid is 1g:40-60ml; preferably, the concentration of concentrated nitric acid is greater than or equal to 6mol / L.
4. The preparation method according to claim 1, Its characteristics are: In step (2), according to Mo 2 The loading amount of C on the modified biological activated carbon is 10-25wt% and the required amount of ammonium molybdate is loaded onto the modified biological activated carbon.
5. The preparation method according to claim 1, Its characteristics are: In step (3), the reaction is carried out at 680-720°C for 2-3 hours.
6. An acidic hydrodeoxygenation catalyst prepared according to the method for preparing an acidic hydrodeoxygenation catalyst according to any one of claims 1 to 5.
7. Use of the hydrodeoxygenation catalyst according to claim 6 in catalyzing the conversion of bio-oil into biofuel.
8. A method for preparing biofuel, Its characteristics are: Biofuel is obtained by taking bio-oil as raw material and carrying out a hydrodeoxygenation reaction under the catalysis of the hydrodeoxygenation catalyst described in claim 6.
9. The preparation method according to claim 8, Its characteristics are: The bio-oil includes jatropha oil.
10. The preparation method according to claim 8, Its characteristics are: The bio-oil, solvent and catalyst are mixed, and then hydrogen is introduced to carry out a hydrodeoxygenation reaction; preferably, the amount of the catalyst is 5-20% of the mass of the bio-oil; preferably, the pressure of the hydrogen is 0.5-4Mpa; preferably, the reaction temperature is 280-360°C, and the reaction time is 3-6h.
Citation Information
Patent Citations
Zirconium phosphate grease hydrodeoxygenation catalyst loaded with transition metal
CN116651476A
Method and apparatus for preparing arene and olefin by means of catalytic hydrogenation coupled with catalytic cracking of bio-fuel
WO2019019539A1