Grain control method for large-size directional column crystal hollow blade of heavy gas turbine
By setting up a follow-up baffle in the wax module and applying a thermal radiation coating, the problem of insufficient temperature gradient control of large-size oriented column crystal blades is solved, the grain consistency and manufacturing efficiency of the blades are improved, and the cost is reduced.
Patent Information
- Application Number
- CN202411186736.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively control the temperature gradient of hollow blades of large-size oriented column crystals, resulting in excessive leaf angle and edge plate crystals, increasing manufacturing difficulty and cost.
A follow-up baffle is installed in the wax module, and a silicate cement thermal radiation coating containing graphite powder is coated on the outer surface of the mold shell to enhance temperature gradient control and ensure the grain growth direction of large-size oriented column crystal blades consistency.
The metallurgical qualification rate of large-size directional column crystal blades is improved, the product scrap rate and manufacturing cost are reduced, and the manufacturing efficiency is improved by about 50%.
Smart Images

Figure CN119057016A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hollow blade casting, in particular to a grain control method for a large-size directional columnar crystal hollow blade of a heavy-duty gas turbine. Background Art
[0002] Ground gas turbine manufacturing has always been recognized as a high-tech product integrating advanced and difficult technologies in multiple disciplines, professions, and fields in the field of heavy equipment manufacturing. It marks the country's technological development level and is an important pillar industry of the national economy of developed countries. At present, the power of advanced heavy-duty gas turbine units is as high as 400MW or more, and the inlet temperature before the turbine is above 1600℃. In order to meet the extreme service conditions of heavy-duty gas turbines, the core high-temperature components of heavy-duty gas turbines, turbine blades, have developed from the initial equiaxed crystals to the current hollow directional columnar crystal blades. Due to the characteristics of blades with no blade body margin, length greater than 300mm, general weight greater than 10kg, complex inner cavity structure, and large heat capacity during solidification, the manufacturing process difficulty of large-size directional columnar crystal blades for heavy-duty gas turbines has increased significantly, especially in the process of directional solidification, the problems of macroscopic blade body grain angle deviation and edge plate impurity caused by cross-section changes and temperature gradient differences in thick edge plate parts are more prominent.
[0003] The existing precision casting technology for high-temperature turbine blades is mainly small-sized directional columnar crystal hollow blades, which are usually within 200mm in height. The temperature gradient during solidification is controllable, with low risk, and it is not easy to have blade body angle deviation and edge plate impurity. The existing technology uses an external follow-up baffle to control the temperature gradient. The existing follow-up external baffle technology is effective for directional hollow blades with a height of less than 200mm. For large-sized directional columnar crystal blades with a height of more than 300mm, the temperature field control is insufficient. In the directional solidification process, the temperature gradient is insufficient and the mushy zone is wide in the stage above 200mm, that is, the part above the edge plate. It is easy to form impurities and the grain growth angle is deviated at this stage. These problems will lead to high scrap rate and high cost of large-sized directional columnar crystal turbine blades. In view of the shortcomings of the metallurgical control technology of large-sized directional columnar crystal blade angle deviation and edge plate impurity, the present invention provides a grain control method for large-sized directional columnar crystal hollow blades of heavy-duty gas turbines to ensure that the macroscopic structure of large-sized directional columnar crystal blades meets the requirements of acceptance specifications. Summary of the invention
[0004] In view of the existing problems, the present invention provides a grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines, which can effectively solve the problems raised in the background technology.
[0005] To solve the above problems, the present invention adopts the following technical solutions:
[0006] A grain control method for a large-size directional columnar crystal hollow blade of a heavy-duty gas turbine comprises the following steps:
[0007] S1. Wax model assembly: fix a center column in the middle of the chassis, fix the top of the center column with a pouring cup, distribute the blade wax models around the circumference of the center column and fix the bottom of the model to the chassis, provide a tenon riser at the top of the blade wax model, connect the pouring cup to the tenon riser on the blade wax model through a runner, and assemble into a wax model set;
[0008] S2, temperature gradient primary treatment: adhere the conformal baffle plate to the center column from bottom to top, and the distance between the conformal baffle plate and the blade wax mold is 50 mm;
[0009] S3, shell preparation: the wax mold after the temperature gradient treatment is shelled at a suitable temperature and humidity, and then dewaxed to prepare a casting shell;
[0010] S4, secondary temperature gradient treatment: a layer of thermal radiation coating is uniformly coated on the outer surface of the conformal baffle shell and the outer surface of the blade shell above the edge plate, and the gap between the conformal baffle shell and the blade shell after the thermal radiation coating is applied is within 20 mm.
[0011] As a further solution of the present invention: the blade wax model is a hollow blade of a heavy-duty gas turbine, and the height of the blade wax model is greater than 300 mm.
[0012] As a further solution of the present invention: the number of blade wax models in the wax model set is three and distributed in a ring array.
[0013] As a further solution of the present invention: the conformal baffles are arranged in plurality along the axial direction of the center column and the distance between adjacent conformal baffles is 80-100 mm.
[0014] As a further solution of the present invention: the shape of one end of the conformal baffle close to the blade wax model is consistent with the shape of the corresponding position of the blade wax model.
[0015] As a further solution of the present invention: the thermal radiation coating is silicate cement containing graphite powder.
[0016] As a further solution of the present invention: the content of graphite powder in the thermal radiation coating is 5%-15% of the content of silicate cement.
[0017] As a further solution of the present invention: the thickness of the thermal radiation coating is 4-6 mm.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention further improves the temperature gradient during directional solidification of large blades by coating the outer shell of the conformal baffle and the outer surface of the blade shell above the edge plate, so as to solve the problems of blade body angle tolerance and edge plate miscellaneous crystals of large-sized directional columnar crystal blades; large-sized directional columnar crystal blades prepared by this method have a high metallurgical qualification rate and a low probability of the appearance of original equiaxed crystals, which comprehensively improves the qualification rate of large-sized directional columnar crystal blades by about 50%, greatly reducing the manufacturing cost of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic flow chart of the control method of the present invention;
[0020] Figure 2 It is a schematic diagram of the medium-sized shell structure of the present invention.
[0021] In the figure: 1. Blade; 2. Chassis; 3. Tenon riser; 4. Center column; 5. Sprue cup; 6. Sprue; 7. Conformal baffle; 8. Thermal radiation coating. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Combination Figure 1 to Figure 2 This embodiment describes a method for controlling grain size of a large-size directional columnar hollow blade of a heavy-duty gas turbine, which comprises the following steps:
[0024] The wax model of the blade 1, as well as the wax models of the chassis 2, the tenon riser 3, the center column 4, the pouring cup 5, and the pouring channel 6 are prepared in advance in the wax mold. After the preparation work is completed, the wax model is assembled. The wax model of the blade 1 is a heavy-duty gas turbine hollow blade 1, and the height of the wax model of the blade 1 is greater than 300 mm.
[0025] Wax model assembly: a center column 4 is fixed in the middle of the chassis 2, the upper end of the center column 4 is fixedly connected to the pouring cup 5, the wax model of the blade 1 is distributed around the circumference of the center column 4 and the lower end is fixed to the chassis 2. Specifically, three wax models of the blade 1 are arranged and distributed in a circular array, the upper end of the wax model of the blade 1 is wax-welded with a tenon riser 3, and the pouring cup 5 is connected to the tenon riser 3 on the wax model of the blade 1 through a runner 6 to assemble into a wax model group;
[0026] Temperature gradient one-time treatment: a conformable baffle 7 is bonded to the middle column 4 from bottom to top. The conformable baffle 7 is a wax sheet. The conformable baffle 7 is arranged in multiple numbers along the axial direction of the middle column 4, and the distance between adjacent conformable baffles 7 is 80-100 mm. The conformable baffles are arranged in parallel, and the distance between the conformable baffle 7 and the wax mold of the blade 1 is 50 mm. The shape of one end of the conformable baffle 7 close to the wax mold of the blade 1 is consistent with the shape of the corresponding position of the wax mold of the blade 1, that is, the circumferential direction of the end face of the conformable baffle 7 away from the middle column 4 is consistent with the curved surface of the blade 1 at the corresponding position;
[0027] Shell preparation: The wax mold after the temperature gradient treatment is made into a shell at a suitable temperature and humidity, and then dewaxed to prepare a casting shell. The shell preparation process adopts a conventional preparation process, which is not specifically described in this example;
[0028] Secondary treatment of temperature gradient: After the casting shell is prepared, a layer of thermal radiation coating 8 is evenly coated on the outer surface of the conformal baffle 7 shell and the outer surface of the blade 1 shell above the edge plate. After the conformal baffle 7 shell is coated with the thermal radiation coating 8, the gap between it and the blade 1 shell is within 20 mm. The gaps between all conformal baffle 7 shells and the blade 1 shells at the corresponding positions are consistent. The edge plate part of the blade 1 shell is usually the place with the lowest temperature gradient and the largest cross-sectional variation. Coating the thermal radiation coating 8 on this part can increase the temperature gradient so as to better control the grains. The blade body is usually relatively smooth and has been controlled by internal and external baffles, which can control the growth direction of the grains.
[0029] In this example, the thermal radiation coating 8 is silicate cement containing graphite powder, that is, graphite powder is added to silicate cement, and solvent water is added to form a slurry, which is applied to the surface of the shell and dried naturally. The content of graphite powder in the thermal radiation coating 8 is 5%-15% of the content of silicate cement. The thickness of the thermal radiation coating 8 is 4-6mm, preferably 5mm. Silicate cement is a black substance that can not only adhere graphite powder to the shell and is resistant to high temperature, but also increase radiation itself. This material is also cheap and easy to obtain, which further reduces costs.
[0030] The working principle of the present invention is: by coating the outer shell of the conformal baffle 7 and the outer surface of the blade 1 shell above the edge plate, the temperature gradient during directional solidification of the large blade 1 is further improved to solve the problem of blade body angle deviation and edge plate miscellaneous crystals of the large-sized directional columnar crystal blade 1; the large-sized directional columnar crystal blade 1 prepared by this method has a high metallurgical qualification rate and a low probability of the original equiaxed crystal appearing, which comprehensively improves the qualification rate of the large-sized directional columnar crystal blade 1 by about 50%, greatly reducing the manufacturing cost of the product.
[0031] It should be noted that, in this article, relational terms are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0032] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines, characterized in that: The steps include: S1. Wax model assembly: fix a center column in the middle of the chassis, fix the top of the center column with a pouring cup, distribute the blade wax models around the circumference of the center column and fix the bottom of the model to the chassis, provide a tenon riser at the top of the blade wax model, connect the pouring cup to the tenon riser on the blade wax model through a runner, and assemble into a wax model set; S2, temperature gradient primary treatment: adhere the conformal baffle plate to the center column from bottom to top, and the distance between the conformal baffle plate and the blade wax mold is 50 mm; S3, shell preparation: the wax mold after the temperature gradient treatment is subjected to shell making at a suitable temperature and humidity, and then dewaxed to prepare a casting shell; S4, secondary temperature gradient treatment: a layer of thermal radiation coating is uniformly coated on the outer surface of the conformal baffle shell and the outer surface of the blade shell above the edge plate, and the gap between the conformal baffle shell and the blade shell after the thermal radiation coating is applied is within 20 mm.
2. The grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 1 is characterized in that: The blade wax model is a hollow blade of a heavy-duty combustion engine, and the height of the blade wax model is greater than 300 mm.
3. The grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 1 is characterized in that: The wax mold group includes three blade wax molds arranged in a circular array.
4. The grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 1 is characterized in that: The conformal baffles are arranged in plurality along the axial direction of the center column, and the distance between adjacent conformal baffles is 80-100 mm.
5. A grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 4, characterized in that: The shape of one end of the conformable baffle close to the blade wax model is consistent with the shape of the corresponding position of the blade wax model.
6. The grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 1 is characterized in that: The heat radiation coating is silicate cement containing graphite powder.
7. A grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 6, characterized in that: The content of graphite powder in the heat radiation coating is 5%-15% of the content of silicate cement.
8. The grain control method for large-size directional columnar crystal hollow blades of heavy-duty gas turbines according to claim 1 is characterized in that: The thickness of the heat radiation coating is 4-6 mm.