Pickled steel welding oxide skin control method
By controlling welding energy and cooling time, the method addresses oxide scale peeling in pickled steel welding, ensuring high-quality welds through precise process adjustments.
Patent Information
- Application Number
- CN202411254332.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods fail to effectively control oxide scale during pickled steel welding, leading to peeling and quality issues in the welding surface, particularly in single-sided welding processes like T-welding and lap welding.
Control the welding process by adjusting the ratio of welding line energy to steel plate thickness and post-weld cooling time to prevent excessive oxide scale formation, using gas shielded single-sided welding with specific parameters for welding current, voltage, and speed to maintain a thin, adherent oxide layer.
Prevents oxide scale peeling and ensures high-quality welding by controlling oxide scale thickness and composition, facilitating smooth progression of subsequent processes.
Smart Images

Figure CN119057174A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pickled steel welding, and in particular to a method for controlling oxide scale in pickled steel welding. Background Art
[0002] In addition to having better strength, pickled steel plates also have advantages such as good surface quality, good cold forming performance and good pitting resistance compared to hot-rolled steel plates. Its surface quality is between hot-rolled and cold-rolled plates, making it an important choice for automobiles and home appliances. Pickling is a surface treatment process that uses the chemical reaction of acid and iron oxide to remove the oxide scale on the surface of hot-rolled steel plates. Normally, there is no oxide on the surface of normal pickled steel.
[0003] At present, there are extensive studies on the control of oxides in the steel rolling process. For example, "Control Technology of Oxide Scale in Hot Strip Rolling. 2009.1" introduces the structure, composition and evolution of surface oxide scale in the hot strip rolling process, and proposes a hot rolling, cooling and coiling technology route that effectively inhibits the growth of oxide scale and reduces the coverage of red oxide scale. Pickling steel will also produce oxides during hot processing. "Method and device for reducing oxide scale formation during hot processing of metals, especially steel (CN93103128.1)" discloses a method for reducing oxide scale formation during hot processing of metals, especially steel, by delivering inert gas through nozzles and devices for protection.
[0004] Arc welding is a type of thermal processing and the main welding method for pickled steel. During welding, a series of changes occur on the surface of the heat-affected zone of the weld: under the action of welding heat, the anti-rust oil on the surface of the steel plate is gradually burned. Because the back of the weld is exposed to the air without protection during welding, the alloy elements in the steel (mainly Fe) are likely to react with the oxygen in the air to produce iron oxides; in the application of pickled steel welding, when single-sided welding (such as T-welding, lap welding), when the welding process is not appropriate, the back of the weld will be severely oxidized and even peeling will occur, affecting the quality of the welding surface and bringing great difficulties to subsequent processes such as painting. At present, there is no effective solution for the control of oxide scale during pickled steel welding. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem that the oxide scale cannot be effectively controlled during the pickling steel welding process in the prior art, and to provide a method for controlling the oxide scale of pickling steel welding. The method effectively controls the oxide scale on the surface of the welding heat affected zone by controlling the welding process, avoids the peeling phenomenon, and thus ensures the welding quality.
[0006] In order to achieve the above object, the present invention provides a method for controlling pickled steel welding scale, the method comprising the following steps:
[0007] (1) The pickled steel plate was welded, and the ratio of the welding line energy E (in J / cm) to the pickled steel plate thickness h (in cm) was controlled to be 1.3×10 4 ~1.9×10 4 ;
[0008] (2) Control cooling after welding to T c Time t c ≤20s, t c The calculation formula is shown in formula (a):
[0009]
[0010] In formula (a), T c is the critical temperature (in the specific embodiment of the present invention) at which FeO is rapidly generated in the pickled steel plate. c =800°C); T0 is the temperature of the pickled steel plate at the beginning of welding (in the specific implementation of the present invention, T0 is room temperature 25°C); λ is the thermal conductivity of the pickled steel plate (in the present invention, λ is 0.42kW / cm·°C); π is 3.14; cρ is the volumetric specific heat capacity of the pickled steel plate (in the present invention, the result of cρ is 5.25J / cm 3 ·℃).
[0011] In the present invention, based on the total weight of the pickled steel plate as 100%, the chemical composition of the pickled steel plate contains: C: 0.05-0.12%, Si≤0.05%, Mn: 1-1.7%, P≤0.02%, S≤0.015%, Nb≤0.1%, Ti≤0.03%, and the rest is Fe and unavoidable impurities.
[0012] The pickled steel welding scale control method of the present invention is mainly aimed at medium-thin pickled steel plates. Furthermore, the pickled steel plates have a thickness h of 0.15 to 0.5 cm.
[0013] In the present invention, for the pickled steel plate of the above thickness, the weld size needs to be controlled during welding to avoid peeling, so the weld depth needs to be controlled to 1 / 3 to 1 / 2 of the pickled steel plate thickness h, so as to ensure a good weld size.
[0014] In order to control the weld depth within the above range, the ratio of welding line energy E to pickled steel plate thickness h (E / h) needs to be controlled to 1.3×10 4 ~1.9×10 4 .
[0015] Since the steel plate is oxidized in the air, the degree of oxidation increases with the increase of temperature and time, mainly iron oxide. Before 400℃, a thin Fe2O3 oxide film is slowly generated, followed by a double oxide film Fe3O4+Fe2O3; at 400-570℃, under the Fe2O3 layer, it grows into a thicker film layer; when the temperature is higher than 575℃, under Fe3O4, FeO begins to form close to the substrate. Since the welding heating process is very fast, the degree of oxidation in the heating stage is relatively light. However, the high temperature residence time after the arc is long, and FeO is quickly generated above 800℃, and it is slower between 800 and 575℃; FeO continues to cool and eutectoid and eutectoid transformation occurs, producing Fe3O4+Fe2O3 until 300℃. The oxide film is composed of a three-layer structure of FeO+Fe3O4+Fe2O3 from the inside to the outside. Therefore, during welding, the stage of cooling to 800℃ after the arc has a major influence on the formation of the oxide layer (especially the thickness). In order to obtain a very thin iron oxide scale, the heating temperature and time must be controlled. The lower the heating temperature and the shorter the heating time, the thinner the iron oxide scale. The adhesion of different iron oxides to the steel base is different. The greater the adhesion, the less likely the oxide will fall off. The breaking stress of FeO+Fe3O4+Fe2O3 is 0.4, 40, and 10MPa respectively. Therefore, when the oxide scale is mainly Fe3O4, the oxide scale is not easy to fall off. Therefore, the main focus of welding should be on controlling the generation of FeO. The less FeO is generated, the better.
[0016] After a lot of research, it is shown that in order to control the amount of FeO generated during the welding of pickled steel plates, it is critical to control the time when the temperature is above 800°C in the welding process. However, the time when the temperature is above 800°C during the welding heating stage is very short and can be ignored. Therefore, the time when the temperature is above 800°C after welding is used as the time when the temperature is above 800°C in the welding process. Therefore, in the present invention, by controlling the cooling time after welding to T c (In the present invention, T c 800℃) time t c , to achieve the corresponding purpose; further preferably, t c ≤20s.
[0017] In the present invention, the calculation formula of the welding line energy E is shown in formula (b):
[0018] E=60UI / v (b)
[0019] In formula (b), I is the welding current (unit: A); U is the welding voltage (unit: V); and v is the welding speed (unit: cm / min).
[0020] Therefore, for the welding of medium and thin pickled steel plates, the ratio of welding line energy E to the thickness of the pickled steel plate h and t cThe main factors are welding current I, welding voltage U and welding speed v, and their main functions are as follows:
[0021] Welding current I: As the welding current I decreases, the heat input decreases, the penetration decreases, and the degree of oxidation on the back of the weld decreases, but too low a current will affect the stability of the arc and the size of the weld; therefore, the appropriate welding current I is 150~270A.
[0022] Welding voltage U: As the welding voltage U decreases, the heat input decreases, the penetration decreases slightly, and the degree of oxidation on the back of the weld decreases. However, too low a voltage will affect the stability of the arc and the size of the weld; the appropriate welding voltage U is 18 to 25V.
[0023] Welding speed v: As the welding speed v increases, the heat input decreases, the penetration decreases, and the degree of oxidation on the back of the weld decreases. However, too fast a welding speed will affect the stability of the arc and the size of the weld; the appropriate welding speed v is 50-70 cm / min.
[0024] Therefore, for the medium-thin pickled steel plate of the present invention, the welding current I, welding voltage U and welding speed v are adjusted during welding to control the welding penetration and the cooling time after welding.
[0025] Generally, before welding, the welding current I, welding voltage U and welding speed v can be roughly selected within the above range according to the specific thickness of the pickled steel plate, and then the E / h and t can be calculated by using the formula. c , the calculated E / h and t c The range required by the present invention needs to be met. If not, the welding current I, welding voltage U and welding speed v are adjusted within the above range so that E / h and t c Meet the requirements of the present invention; then weld according to the welding current I, welding voltage U and welding speed v that meet the requirements, so that the ratio of welding line energy E to the pickled steel plate thickness h is 1.3×10 4 ~1.9×10 4 , and t c ≤20s, so that the weld is well formed, the weld depth is controlled to be 1 / 3 to 1 / 2 of the thickness h of the pickled steel plate, the thickness and composition of the oxide scale on the back of the weld can be well controlled, and oxidation peeling can be avoided.
[0026] The type of welding in the present invention is single-sided welding. Furthermore, in the present invention, gas shielded welding is used to perform single-sided welding on the pickled steel plate.
[0027] Among them, the welding method is single-pass cladding, T-type welding or lap welding.
[0028] In the present invention, suitable process conditions are determined in combination with the thickness of the pickled steel plate for single-sided welding, ensuring that the heating time on the back side of the weld is reduced, thereby controlling the thickness of the oxide scale on the back side of the weld, avoiding the oxide scale from curling up or falling off, and creating good conditions for the smooth progress of subsequent processes of the workpiece. This scheme creates conditions for the production quality and efficiency of subsequent processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of welding types;
[0030] Figure 2 is a back view of the weld of Example 4;
[0031] Figure 3 is a scanning electron microscope image of a cross section of the oxide layer at the weld of Example 4;
[0032] Figure 4 This is a picture showing the peeling of the back of the weld in comparative example 1;
[0033] Figure 5 This is a scanning electron microscope image of the cross-section of the oxide layer near the peeling area of the weld in comparative example 1. DETAILED DESCRIPTION
[0034] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0035] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0036] The welding types in the following embodiments are all single-sided welding, and gas shielded welding is used for single-sided welding; Figure 1 The lap welding shown in b in the figure is used in the other embodiments and comparative examples. Figure 1 Single pass weld as shown in a.
[0037] Taking the total weight of the pickled steel plate as 100%, the chemical composition of the pickled steel plate includes: C: 0.08%, Si: 0.03%, Mn: 1.4%, P: 0.010%, S: 0.009%, Nb: 0.05%, Ti: 0.02%, and the rest is Fe and inevitable impurities.
[0038] Example 1
[0039] (1) The pickled steel plate without oxide scale on the surface was welded. The thickness of the pickled steel plate was h 0.18 cm, the welding current I was 160 A, the welding voltage U was 18 V, and the welding speed v was 70 cm / min. The welding line energy E was 2469 J / cm2 when substituted into formula (b). The ratio of the welding line energy E to the thickness of the pickled steel plate h was 1.37×10 4 ;
[0040] E=60UI / v (b)
[0041] (2) According to formula (a), the post-weld cooling to the critical temperature T c (800℃) time t c is 11s,
[0042]
[0043] In formula (a), the temperature T0 of the pickled steel plate at the beginning of welding is 25°C, π is 3.14, the thermal conductivity λ of the pickled steel plate is 0.42kW / cm·°C, and the volume specific heat capacity cρ of the pickled steel plate is 5.25J / cm 3 ℃;
[0044] Among them, the weld depth is 0.07cm.
[0045] The specific process parameters of Examples 1-5 are shown in Table 1. Comparative Examples 1-2 are implemented according to the method of Example 1, and the process parameters are different from those of Example 1. The specific process parameters are shown in Table 1 (the critical temperature T in Examples 2-5 and Comparative Examples 1-2 is c The temperature of the pickled steel plate at the beginning of welding is 800℃, and the temperature T0 of the pickled steel plate at the beginning of welding is 25℃. The peeling condition after welding is shown in Table 1.
[0046] Table 1
[0047]
[0048]
[0049] From the results in Table 1, it can be seen that in Examples 1 to 5, pickled steel plates with thicknesses of 0.18 cm, 0.25 cm, 0.3 cm, 0.38 cm and 0.45 cm were welded according to the technical solution of the present invention, and the welds had no defects and no peeling occurred;
[0050] After welding in Comparative Examples 1 and 2, peeling occurred on the back of the weld.
[0051] Test Case
[0052] Observe the back of the weld of Example 4 with naked eyes. Figure 2As shown; and prepare the cross-section sample of the weld in Example 4, grind and polish it, and observe the oxide layer under FEIQuanta400 scanning electron microscope. The results are as follows Figure 3 As shown ( Figure 2 This is the back side of the weld in Example 4. Figure 3 4 is the scanning electron microscope analysis result of the cross section of the oxide layer at the weld of Example 4). The same method is used to observe the peeling of the back of the weld of Comparative Example 1 and the cross section of the oxide layer near the peeling part of the weld. Figure 4-5 As shown ( Figure 4 This is the peeling situation on the back of the weld in comparative example 1. Figure 5 This is the scanning electron microscope analysis result of the cross section of the oxide layer near the peeling area of the weld in comparative example 1).
[0053] The FEI Quanta 400 scanning electron microscope was used to perform energy spectrum analysis on the skinning layer components of Example 4 and Comparative Example 1. The results are shown in Table 2.
[0054] Table 2
[0055]
[0056] Note: wt%-weight percentage, at%-atomic percentage.
[0057] Combination Figure 2-5 And Table 2, such as Figure 2-3 From the analysis results of Example 4 shown in Table 3, it can be seen that only a single layer of oxide scale is produced on the back of the weld in Example 4; according to the atomic numbers of O and Fe in Table 2 (O is 57.15%, Fe is 42.09%), it can be inferred that the oxide layer is mainly Fe3O4, which has a strong adhesion to the steel base and is not easy to peel (detach or warp);
[0058] like Figure 4-5 According to the analysis results of comparative example 1 shown in Table 2, a weld nodule appeared on the back of the weld of comparative example 1, and peeling occurred on the back of the weld; a microscopic analysis of the cross section of the oxide layer near the peeling position showed that the oxide layer was a double-layer iron oxide; according to the atomic ratio of O to Fe in comparative example 1 in Table 2, it can be seen that the O in the inner layer is 52.44% and the Fe is 47.56%, which can be inferred to be mainly FeO; while the O in the outer layer is 53.79% and the Fe is 45.47%, which can be inferred to be mainly Fe3O4; the inner oxide layer mainly composed of FeO has low adhesion to the steel base, so it is easy to peel.
[0059] According to the above results, by adopting the scheme of the present invention, the thickness and composition of the oxide scale on the back of the weld can be well controlled when welding the pickled steel plate, and oxidation peeling can be avoided.
[0060] It should be understood that parts not elaborated in detail in this specification belong to the prior art.
[0061] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for controlling pickled steel welding scale, characterized in that: The pickled steel welding scale control method comprises the following steps: (1) Weld the pickled steel plate and control the ratio of welding line energy E to the thickness h of the pickled steel plate to be 1.3×10 4 ~1.9×10 4 ; (2) Control cooling after welding to T c Time t c ≤20s, t c The calculation formula is shown in formula (a): In formula (a), T c is the critical temperature; T0 is the temperature of the pickled steel plate at the beginning of welding; λ is the thermal conductivity of the pickled steel plate; cρ is the volume specific heat capacity of the pickled steel plate.
2. The method for controlling pickled steel welding scale according to claim 1, characterized in that: Taking the total weight of the pickled steel plate as 100%, the chemical composition of the pickled steel plate includes: C: 0.05-0.12%, Si≤0.05%, Mn: 1-1.7%, P≤0.02%, S≤0.015%, Nb≤0.1%, and Ti≤0.03%.
3. The method for controlling pickled steel welding scale according to claim 1 or 2, characterized in that: The thickness h of the pickled steel plate is 0.15 to 0.5 cm.
4. The method for controlling pickled steel welding scale according to claim 1, characterized in that: The calculation formula of the welding line energy E is shown in formula (b): E=60UI / v (b) In formula (b), I is the welding current; U is the welding voltage; and v is the welding speed.
5. The method for controlling pickled steel welding scale according to claim 4, characterized in that: The welding current I is 150~270A.
6. The method for controlling pickled steel welding scale according to claim 4, characterized in that: The welding voltage U is 18~25V.
7. The method for controlling pickled steel welding scale according to claim 4, characterized in that: The welding speed v is 50-70 cm / min.
8. The method for controlling pickled steel welding scale according to claim 1, characterized in that: The weld depth is 1 / 3 to 1 / 2 of the pickled steel plate thickness h.
9. The method for controlling pickled steel welding scale according to claim 1, characterized in that: The type of welding is single-sided welding.
10. The method for controlling pickled steel welding scale according to claim 1 or 9, characterized in that: Gas shielded welding is used for single-side welding of pickled steel plates.