Composite brazing filler metal for welding carbon-based material and titanium-based alloy, brazing filler metal piece and preparation method and brazing method of brazing filler metal piece

By using composite solder of TiH2, Nb and AgCu28, the high thermal expansion, low strength and brittle compound layer problems of AgCu solder when welding carbon-based materials and titanium-based alloys are solved, and the high temperature mechanical properties and welding accuracy are improved. Provides better joint performance.

CN119057308AActive Publication Date: 2024-12-03SUN YAT SEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411548312.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-12-03
Estimated Expiration
2044-11-01

AI Technical Summary

Technical Problem

When welding carbon-based materials and titanium-based alloys, existing AgCu-based solder materials have problems with high thermal expansion coefficient, low joint strength, low temperature mechanical properties and brittle compound layers, resulting in poor welding accuracy and performance.

Method used

The solder sheet was prepared by mechanical ball mill mixing and using the composite solder material including 3 wt.%~9 wt.% TiH2, 20 wt.%~50 wt.% Nb and a margin of AgCu28. Characteristics of Nb particles and TiH2 powder, control the flow and high temperature performance of solder, reduce the thermal expansion coefficient and chemical reaction.

Benefits of technology

It significantly improves the strength and high-temperature mechanical properties of the joint, reduces the formation of brittle compounds, improves the welding accuracy and shear strength of the joint, and significantly improves the performance under both room temperature and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the field of welding, in particular to a composite brazing filler metal for welding a carbon-based material and a titanium-based alloy, a brazing filler metal piece and a preparation method and a brazing method of the brazing filler metal piece. The composite brazing filler metal provided by the invention is used for brazing a carbon-based material and a titanium-based material, has few brittle compounds, and has high joint strength and high-temperature mechanical properties; the bottleneck problems that when a carbon-based material and titanium-based alloy connecting component is prepared through traditional AgCu brazing filler metal brazing, the residual stress of a connector is large, the using temperature is low, more brittle compounds exist, and brazing filler metal excessively flows are solved, the performance of the connecting component is poor, and the welding precision of the connecting component is improved. Tests show that the composite brazing filler metal is used for welding a carbon-based material and a titanium-based alloy, the room-temperature shear strength of a joint is high and is 2-3 times that of an AgCu28 brazing filler metal joint under the same condition, the shear strength of the joint is not reduced at the high temperature of 600 DEG C, and the joint still keeps high strength at the temperature of 800 DEG C (close to the welding temperature).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of welding, in particular to a composite brazing filler metal and a brazing filler metal sheet for welding carbon-based materials and titanium-based alloys, and a preparation method and a brazing method thereof. Background Art

[0002] Carbon-based materials and titanium-based alloys are widely used in the fields of automobiles, electronic devices, petrochemicals, and aerospace. In actual engineering applications, carbon-based materials and titanium-based alloys are often connected to form structural and functional integrated connection components to meet the stringent requirements of the service environment. For example, in deep-sea oil and gas pipelines, graphite and titanium alloy connection components can be used as sealing static rings; in aircraft engines, SiBCN ceramics and Ti 2 The AlNb connecting component can be used as a nozzle transition joint.

[0003] At present, brazing connection using AgCu-based solder is one of the main methods for preparing carbon-based and titanium-based composite components. However, the thermal expansion coefficient of AgCu solder is high, and there is a high residual stress in the joint after welding, and the joint strength is low; the melting point of AgCu solder is low, and the oxidation resistance of Cu-based solid solution is poor, which leads to poor high-temperature mechanical properties of the joint; Cu and Ti in AgCu solder have a strong reaction tendency, which leads to a large diffusion of Cu in the solder into the titanium-based alloy and a large dissolution of Ti into the solder, thereby forming a continuous brittle compound layer and deteriorating the joint performance; the high chemical affinity of Cu and Ti leads to excessive flow of solder on the surface of titanium-based materials, affecting the welding accuracy and aesthetics; the preferential spreading of solder on titanium-based materials also leads to unwelded and unwetted phenomena on the surface of carbon-based materials. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a composite brazing filler metal, a brazing filler metal sheet, and a preparation method and a brazing method for welding carbon-based materials and titanium-based alloys. The composite brazing filler metal provided by the present invention is used for brazing carbon-based materials and titanium-based materials, has less brittle compounds, and has high joint strength and high-temperature mechanical properties.

[0005] The present invention provides a composite brazing filler metal for welding carbon-based materials and titanium-based alloys, comprising:

[0006] 3 wt.%~9 wt.% TiH 2 ;

[0007] 20 wt.%~50 wt.% Nb;

[0008] The balance is AgCu28.

[0009] Preferably, the composite brazing filler metal for welding the carbon-based material and the titanium-based alloy comprises:

[0010] 4 wt.%~8 wt.% TiH 2 ;

[0011] 25 wt.%~35 wt.% Nb;

[0012] The balance is AgCu28.

[0013] More preferably, the composite brazing filler metal for welding the carbon-based material and the titanium-based alloy comprises:

[0014] 5 wt.%~7 wt.% TiH 2 ;

[0015] 28 wt.%~32 wt.% Nb;

[0016] The balance is AgCu28.

[0017] The composite brazing filler metal for welding carbon-based materials and titanium-based alloys of the present invention comprises TiH 2 , Nb and AgCu28; wherein the Nb added to the composite solder is Nb particles with a mesh size of 100-200 meshes. Nb particles are high-melting-point metals and do not melt during the brazing process, but are retained in the weld in the form of a skeleton. The liquid phase of the solder can be retained in the welding area through capillary action to avoid excessive flow of the solder and improve the forming accuracy. At the same time, at high temperatures, Nb can act as a high-temperature skeleton to alleviate the softening of the brazing seam, thereby improving the high-temperature mechanical properties of the joint. In addition, the Nb particles added to the composite solder have the characteristics of a low thermal expansion coefficient, which can reduce the thermal expansion coefficient of the solder, reduce the thermal expansion difference between the solder and the carbon-based material, reduce the joint stress, and improve the joint strength.

[0018] The TiH added to the composite solder of the present invention 2 TiH with mesh number of 250~300 2 The TiH 2 The powder can decompose during the heating process of welding and the first insulation stage to form evenly distributed Ti particles and precipitate H 2 .H 2 It has a reducing effect and can clean the oxides on the surface of Nb powder and AgCu28 powder, thereby improving the welding quality. In the second insulation stage of welding, the evenly distributed Ti particles dissolve in the AgCu28 liquid phase, thereby achieving uniform wetting of the liquid phase to the carbon-based material; at the same time, the Ti particles can reduce the chemical concentration difference between the brazing filler metal and the titanium-based material, inhibit the dissolution of the titanium-based material, and reduce brittle compounds.

[0019] The AgCu28 added to the composite solder of the present invention is AgCu28 solder powder with a mesh size of 200 to 300 meshes. The Cu element of the AgCu28 solder powder can react with TiH2 The Ti in the powder can react to form Ti-Cu compounds, eliminating the Cu-based solid solution with poor oxidation resistance and causing the liquid phase composition to deviate from the low-melting point eutectic, thereby increasing the melting point of the weld; while the Nb particles can serve as nucleation sites for the Ti-Cu compounds to achieve uniform distribution of the Ti-Cu compounds, thereby turning waste into treasure and using brittle compounds to strengthen the joint.

[0020] The composite brazing filler metal provided by the present invention is a composite brazing filler metal for welding carbon-based materials and titanium-based alloys. The carbon-based material includes graphite, SiBCN ceramics or SiC ceramics; the titanium-based alloy includes TA2, TC4, TiAl, TC18 or Ti 2 In some embodiments of the present invention, the carbon-based material is preferably SiBCN ceramic and the titanium-based alloy is preferably Ti 2 In some other embodiments of the present invention, the carbon-based material is preferably SiC ceramic and the titanium-based alloy is preferably Ti 2 AlNb.

[0021] The present invention provides a method for preparing the composite solder, comprising the following steps: 2 , Nb and AgCu28 are ground to obtain the composite solder; the TiH 2 , Nb and AgCu28 are the same as above, and will not be repeated; the grinding speed is 150 rpm~300 rpm, and the grinding time is 30 min~60 min. 2 The powder, Nb powder and AgCu28 solder powder are mechanically ball-milled to obtain the composite solder, and the mechanical ball-milling mixing process comprises: mechanically ball-milling for 30 min to 60 min at a speed of 150 rpm to 300 rpm in a planetary ball mill; using anhydrous ethanol as a mixing medium; using ZrO2 with a diameter of 1 mm to 3 mm; 2 Or agate is used as grinding balls; the ball-to-material mass ratio range includes (2~4):1.

[0022] The present invention also provides a solder sheet, which is made from the composite solder described in any of the above technical solutions. The solder sheet of the present invention has a thickness of 100 μm to 300 μm, preferably 200 μm.

[0023] The present invention also provides a method for preparing a solder sheet as described in any of the above technical solutions, comprising the following steps: pressing the above composite solder to obtain a solder sheet; the pressure of the pressing is 2 MPa to 5 MPa. Specifically, the present invention adds the composite solder to a mold for pre-pressing and forming to obtain a preformed solder sheet; the pressure range of the pre-pressing and forming is 2 MPa to 5 MPa.

[0024] The present invention also provides a method for welding a carbon-based material and a titanium-based alloy, comprising the following steps: placing the brazing sheet described in any of the above technical solutions on the surface to be welded of the carbon-based material and the titanium-based alloy, and performing heat treatment. Specifically, the brazing sheet, the carbon-based material and the titanium-based alloy are assembled, and during assembly, the brazing sheet is placed on the surface to be welded of the carbon-based material and the titanium-based alloy, and heat treatment is performed. The brazing sheet, the carbon-based material and the titanium-based alloy described in the present invention are the same as those described above and will not be described in detail.

[0025] More specifically, the above-mentioned brazing sheet, carbon-based material and titanium-based alloy are assembled. During assembly, the brazing sheet is placed on the surface to be welded of the carbon-based material and the titanium-based alloy, and heat treatment is performed. The heat treatment is specifically: heating to 700°C~750°C and keeping warm for 20 min~40 min, then heating to 800°C~860°C and keeping warm for 30 min~60 min.

[0026] In certain embodiments of the present invention, the above-mentioned brazing sheet, carbon-based material and titanium-based alloy are assembled. During assembly, the brazing sheet is placed on the surface to be welded of the carbon-based material and the titanium-based alloy, and heat treatment is performed. The heat treatment is specifically as follows: heating to 700°C~750°C at a heating rate of 8°C / min~12°C / min and keeping warm for 20 min~40 min, then heating to 800°C~860°C at a heating rate of 3°C / min~5°C / min and keeping warm for 30 min~60 min, and finally cooling to below 250°C at a cooling rate of 3°C / min~5°C / min to complete precision welding.

[0027] The present invention provides a composite solder, a solder sheet, and a preparation method and a brazing method for welding carbon-based materials and titanium-based alloys. The composite solder provided by the present invention is used for brazing carbon-based materials and titanium-based materials. It has less brittle compounds, high joint strength and high-temperature mechanical properties, and solves the bottleneck problems of large joint residual stress, low operating temperature, many brittle compounds, excessive flow of solder, etc. in the preparation of carbon-based materials and titanium-based alloy connection components by traditional AgCu solder brazing, thereby improving the poor performance of the connection components and the welding accuracy. Experiments show that the composite solder of the present invention can be used for brazing SiBCN and Ti 2 AlNb welding is still used for SiC and Ti 2 For AlNb welding, the room temperature shear strength of the joint can reach more than 65 MPa, which is three times that of the AgCu28 solder joint under the same conditions. In addition, the shear strength of the joint does not decrease at a high temperature of 600°C, and it still maintains a high strength at 800°C (close to the welding temperature). BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The microstructure of the joint of AlNb alloy at 50 micron scale;

[0029] Figure 2 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The microstructure of the joint of AlNb alloy at 10 micron scale;

[0030] Figure 3 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The joint microstructure and mapping of AlNb alloy at 20 micron scale;

[0031] Figure 4 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The microstructure of the joint of AlNb alloy at 5 micron scale;

[0032] Figure 5 The composite solder for brazing Ti in Example 2 of the present invention 2 The microstructure morphology of the joint between AlNb and SiC;

[0033] Figure 6 The AgCu28 solder of the present invention is used to braze Ti 2 Joint microstructure morphology of AlNb and SiC. DETAILED DESCRIPTION

[0034] The present invention discloses a composite brazing material, a brazing sheet, a preparation method thereof, and a brazing method for welding carbon-based materials and titanium-based alloys. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.

[0035] The present invention will be further described below in conjunction with embodiments:

[0036] Example 1

[0037] The carbon-based material is SiBCN ceramic, and the titanium-based alloy is Ti 2 AlNb alloy, the carbon-based material and the titanium-based alloy are precisely welded by using a composite brazing filler metal, wherein the composite brazing filler metal is 300 mesh TiH 2The powder is obtained by ball milling 30 wt.% of 200 mesh Nb powder and 200 mesh AgCu28 brazing powder; the ball milling mixing process includes: mechanical ball milling at a speed of 200 rpm for 45 min in a planetary ball mill; using anhydrous ethanol as a mixing medium; using a ZrO 2 As grinding balls; ball-to-material mass ratio range includes 3:1.

[0038] The composite solder is pre-pressed to obtain a solder sheet with a thickness of 200 μm; the pressure range of the pre-pressing treatment includes 2.5 MPa. The pre-formed solder sheet and the surface-polished and cleaned carbon-based material and titanium-based alloy are assembled, and the pre-formed solder sheet is placed on the surface to be welded during assembly; the welding system is: heating to 750°C at a heating rate of 10°C / min, keeping warm for 20 min, heating to 820°C at a heating rate of 3°C / min and keeping warm for 30 min, cooling to below 250°C at a cooling rate of 3°C / min, and completing precision welding.

[0039] like Figure 1~Figure 4 As shown, Figure 1 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The morphology of the joint structure of AlNb alloy at 50 micron scale. Figure 2 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The morphology of the joint structure of AlNb alloy at 10 micron scale. Figure 3 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 The joint structure morphology and mapping diagram of AlNb alloy at 20 micron scale. Figure 4 The composite brazing material for brazing SiBCN ceramic and Ti according to Example 1 of the present invention 2 Joint microstructure morphology of AlNb alloy at 5 micron scale.

[0040] The room temperature shear strength of the joint obtained above is 69±9 MPa, which is three times that of the AgCu28 solder joint under the same conditions (24±3MPa). In addition, the shear strength of the joint does not decrease at a high temperature of 600°C, and it still maintains a strength of 24±1 MPa at 800°C (close to the welding temperature).

[0041] Example 2

[0042] Carbon-based materials are SiC and titanium-based alloys are Ti 2 AlNb, the carbon-based material and the titanium-based alloy are precisely welded by using a composite brazing filler metal, wherein the composite brazing filler metal is 300 mesh TiH 2The powder is obtained by ball milling 30wt.% of 200-mesh Nb powder and 200-mesh AgCu28 brazing powder; the ball milling mixing process includes: mechanical ball milling at a speed of 300 rpm for 60 min in a planetary ball mill; using anhydrous ethanol as a mixing medium; using agate with a diameter of 3 mm as a grinding ball; and the ball-to-material mass ratio ranges from 2:1.

[0043] The composite solder is subjected to pre-pressing and forming treatment to obtain a solder sheet with a thickness of 200 μm; the pressure range of the pre-pressing and forming treatment includes 3 MPa. The pre-formed solder sheet is assembled with the surface-polished and cleaned carbon-based material and titanium-based alloy, and the pre-formed solder sheet is placed on the surface to be welded during assembly; the welding system is: heating to 750°C at a heating rate of 10°C / min, keeping warm for 20 min, heating to 820°C at a heating rate of 3°C / min and keeping warm for 30 min, cooling to below 250°C at a cooling rate of 3°C / min, and completing precision welding.

[0044] like Figure 5 and Figure 6 As shown, Figure 5 The composite solder for brazing Ti in Example 2 of the present invention 2 The joint structure morphology of AlNb and SiC. Figure 6 The AgCu28 solder of the present invention is used to braze Ti 2 The joint structure morphology of AlNb and SiC. Figure 5 and Figure 6 It can be seen that the composite solder of Example 2 of the present invention is suitable for brazing Ti 2 The amount of brittle compounds in the joint of AlNb and SiC is greatly reduced, and the room temperature shear strength of the obtained joint is 65±4 MPa, and the strength of the joint does not decrease under high temperature conditions of 600℃.

[0045] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A composite brazing filler metal for welding carbon-based materials and titanium-based alloys, characterized in that: include: 3 wt.%~9 wt.% TiH2; 20 wt.%~50 wt.% Nb; The balance is AgCu28.

2. The composite brazing filler metal for welding carbon-based materials and titanium-based alloys according to claim 1, characterized in that: include: 4 wt.%~8 wt.% TiH2; 25 wt.%~35 wt.% Nb; The balance is AgCu28.

3. The composite brazing filler metal for welding carbon-based materials and titanium-based alloys according to claim 1, characterized in that: The mesh number of the TiH2 is 250-300 mesh; The mesh number of the Nb is 100-200 mesh; The mesh size of the AgCu28 is 200-300 meshes.

4. The composite brazing filler metal for welding carbon-based materials and titanium-based alloys according to any one of claims 1 to 3, characterized in that: The carbon-based material includes graphite, SiBCN ceramic or SiC ceramic; The titanium-based alloy includes TA2, TC4, TiAl, TC18 or Ti2AlNb.

5. A solder sheet, characterized in that: It is made from the composite solder described in any one of claims 1 to 4.

6. The solder sheet according to claim 5, characterized in that: The thickness of the solder sheet is 100 μm to 300 μm.

7. The method for preparing a solder sheet according to claim 5 or 6, characterized in that: The following steps are involved: Pressing the composite solder into a shape to obtain a solder sheet; The pressing pressure is 2 MPa to 5 MPa.

8. A method for welding carbon-based materials and titanium-based alloys, characterized in that: The following steps are involved: The brazing material sheet according to claim 5 or 6 is placed on the surfaces to be welded of the carbon-based material and the titanium-based alloy, and subjected to heat treatment.

9. The welding method according to claim 8, characterized in that: The heat treatment is specifically: heating to 700°C-750°C and keeping the temperature for 20 min-40 min, then heating to 800°C-860°C and keeping the temperature for 30 min-60 min.

10. The welding method according to claim 8, characterized in that: The heat treatment is specifically as follows: heating to 700°C~750°C at a heating rate of 8°C / min~12°C / min and keeping warm for 20 min~40 min, then heating to 800°C~860°C at a heating rate of 3°C / min~5°C / min and keeping warm for 30 min~60 min, and finally cooling to below 250°C at a cooling rate of 3°C / min~5°C / min.

Citation Information

Patent Citations

  • Solder, preparation method thereof and method for connecting sapphire and niobium or niobium alloys by using solder

    CN103056553A

  • High-entropy alloy brazing filler metal for connecting TiAl alloy and silicon nitride ceramic and connecting method of high-entropy alloy brazing filler metal

    CN115091076A

  • Arc welding method for galvanized steel sheets and blowhole preventive for welding

    JP1992009280A