Lightweight compartment bottom plate for new energy vehicle and manufacturing method of lightweight compartment bottom plate
By dissolving the hot pressing composite technology of poplar and eucalyptus veneer and aramid paper honeycomb materials, a high-strength, low-density lightweight car base plate was prepared, which solved the problem that wooden car base plates in the existing technology was difficult to achieve lightweight, and improved the improvement of The endurance of new energy vehicles.
Patent Information
- Application Number
- CN202411284388.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
AI Technical Summary
When the existing wooden and bamboo car base plates meet the structural mechanical performance requirements, it is difficult to achieve a lightweight design and cannot meet the lightweight needs of new energy vehicles.
The mixed composite board is prepared by releasing poplar and eucalyptus veneer through linear convex tooth needle rollers to form cracks, combined with aramid paper honeycomb material and phenolic resin adhesive film paper, and a mixed composite board is prepared through hot pressing process to form high-strength and low-density Lightweight car base plate.
The weight reduction and mechanical performance improvement of the car base plate have been achieved, and the load-bearing capacity and endurance of new energy vehicles have been improved.
Smart Images

Figure CN119057880A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wood-based panels, and in particular relates to a lightweight carriage floor for a new energy vehicle and a manufacturing method thereof. Background Art
[0002] With the rapid development of new energy vehicles, lightweighting has become a key factor in improving vehicle endurance. As the main load-bearing component of the car, the car floor also needs to respond to the lightweight requirements of new energy vehicles and reduce the weight of the material. Existing wooden and bamboo car floors lack lightweight structural design when meeting the requirements of structural mechanical performance, and it is difficult to meet the requirements for lightweight car floors. Therefore, there is an urgent need for a lightweight car floor for new energy vehicles and a manufacturing method thereof. Summary of the invention
[0003] The purpose of the present invention is to provide a lightweight car floor for new energy vehicles and a manufacturing method thereof to solve the above-mentioned problems.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] A method for manufacturing a lightweight car floor for a new energy vehicle comprises the following steps:
[0006] Step 1: Make a reorganized table panel;
[0007] Step 2: Take a specified number of wood veneers and apply glue to the combination, set an aramid paper honeycomb material between two adjacent wood veneers, and obtain a hybrid composite board after hot pressing and fixing;
[0008] Step 3, placing adhesive film on the upper and lower surfaces of the hybrid composite board;
[0009] Step 4: Cover the reconstructed surface board on the upper and lower surfaces of the hybrid composite board with the adhesive paper, and then fix them into shape by hot pressing.
[0010] Preferably, in the step 1, the reconstituted surface board is made of a poplar-eucalyptus mixed board formed by mixing and pressing a debonded poplar veneer and a debonded eucalyptus veneer;
[0011] The debonded poplar veneer is formed by rolling and debonding the poplar veneer with a linear convex tooth needle roller, so that cracks of uniform length are formed in the direction of the grain of the poplar veneer.
[0012] The debonded eucalyptus veneer is formed by rolling and debonding a poplar veneer with a linear convex tooth needle roller, so that cracks of uniform length are formed in the eucalyptus veneer in the direction of the grain;
[0013] The poplar-eucalyptus mixed board is obtained by dipping any number of debonded poplar veneers and any number of debonded eucalyptus veneers in glue, drying, assembling and hot pressing to obtain the reconstituted surface board.
[0014] Preferably, the ratio of the number of the debonded poplar veneers to the number of the debonded eucalyptus veneers in the poplar-eucalyptus hybrid board is 1:1.
[0015] Preferably, in the poplar-eucalyptus mixed board, the debonded poplar veneer and the debonded eucalyptus veneer are arranged at intervals.
[0016] Preferably, in the poplar-eucalyptus mixed board, the outer surface of the poplar-eucalyptus mixed board is the debonded poplar veneer.
[0017] Preferably, the poplar-eucalyptus mixed board has a thickness not exceeding 3 mm.
[0018] Preferably, in step 2, the wood veneer is selected to be a poplar veneer or a eucalyptus veneer.
[0019] Preferably, the hybrid composite board comprises three wood veneers, and the hybrid composite board is a structure of all poplar, all eucalyptus, or a mixed structure of poplar and eucalyptus;
[0020] The poplar-eucalyptus mixed structure is one of poplar, eucalyptus, poplar mixed structure or eucalyptus, poplar, eucalyptus mixed structure.
[0021] Preferably, the thickness of the aramid paper honeycomb material is 3 mm, and the thickness of the adhesive film paper is 0.2 mm.
[0022] Preferably, the crack thickness of the debonded poplar veneer matches the thickness of the debonded poplar veneer, and the crack thickness of the debonded eucalyptus veneer matches the thickness of the debonded eucalyptus veneer;
[0023] The length of the crack is 10-30 mm, the width is 0.1-0.5 mm, the lateral spacing of the crack is less than 2 mm, and the longitudinal spacing is 5-30 mm.
[0024] Preferably, the dipping is performed by a pressurized dipping method, and the pressure is controlled to be 3.0-4.0 MPa.
[0025] Preferably, the honeycomb cell side length of the aramid paper honeycomb material is 3±0.5 mm, and the honeycomb density is 45±5 kg / m 3 ;
[0026] The adhesive film paper is phenolic resin adhesive film paper, and the weight of the adhesive film paper base paper is 100-120g / m 2 , the phenolic resin glue impregnation amount is 180%-220%.
[0027] Preferably, in step three, the hot pressing temperature is 140° C., the hot pressing time is 1.9 min / mm, and the pressure is set to 0.8-1.2 MPa.
[0028] A lightweight car floor for new energy vehicles is manufactured based on the above-mentioned method for manufacturing a lightweight car floor for new energy vehicles.
[0029] Compared with the prior art, the present invention has the following advantages and technical effects:
[0030] The present invention adopts linear convex tooth needle roller to roll and decompress wood veneer to form cracks that penetrate the thickness and are uniform in length. The obtained decomposed veneer not only improves the roughness of the veneer, increases the amount of glue impregnation, and can improve the bonding strength, but also disperses the stress during hot pressing, reduces local stress concentration, and enhances the mechanical properties. After the decomposed veneer is impregnated with glue, dried, and other operations, a high-strength reconstructed surface board is obtained; for the core board, poplar and eucalyptus veneers are mixed with aramid paper honeycomb materials using specific composite methods and different hot pressing processes to form a lightweight composite board with a hollow structure; finally, under the composite of phenolic resin film paper, the surface board and the core board are hot pressed under different hot pressing processes to obtain a mixed composite board.
[0031] Compared with the prior art, the lightweight car floor for new energy vehicles prepared by the present invention achieves the required mechanical properties of the car floor while reducing the weight of the floor. The product has a higher strength-to-weight ratio and maximizes the lightness and high strength of the material properties of poplar and eucalyptus wood themselves, which helps to improve the carrying capacity and endurance of new energy vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative labor:
[0033] Figure 1 It is a process flow chart of the present invention;
[0034] Figure 2 It is a schematic diagram of the structure of the present invention;
[0035] Among them, 1. Reconstructed surface board; 2. Film paper; 3. First layer of veneer; 4. Aramid paper honeycomb material; 5. Second layer of veneer; 6. Third layer of veneer. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0038] Reference Figure 1 to Figure 2 The present invention discloses a method for manufacturing a lightweight car floor for a new energy vehicle, comprising the following steps:
[0039] Step 1: Make a reorganized table plate 1;
[0040] Step 2: Take a specified number of wood veneers and apply glue to the combination, set an aramid paper honeycomb material 4 between two adjacent wood veneers, and obtain a hybrid composite board after hot pressing and fixing;
[0041] Step 3: placing adhesive film 2 on the upper and lower surfaces of the hybrid composite board;
[0042] Step 4: Cover the reconstructed surface plate 1 on the upper and lower surfaces of the mixed composite plate with the adhesive film paper 2, and then fix them into shape by hot pressing.
[0043] The present invention adopts linear convex tooth needle roller to roll and fluff wood veneer to form cracks that penetrate the thickness and are uniform in length. The obtained fluffed veneer not only improves the roughness of the veneer, increases the amount of glue impregnation, and can improve the bonding strength, but also disperses the stress during hot pressing, reduces local stress concentration, and enhances the mechanical properties. The fluffed veneer is then subjected to glue impregnation, drying and other operations to obtain a high-strength reconstructed surface board 1; for the core board, poplar and eucalyptus veneers are mixed and composited with aramid paper honeycomb materials 4 using specific composite methods and different hot pressing processes to form a lightweight composite board with a hollow structure; finally, under the composite of phenolic resin film paper, the surface board and the core board are hot pressed under different hot pressing processes to obtain a mixed composite board.
[0044] Compared with the prior art, the lightweight car floor for new energy vehicles prepared by the present invention achieves the required mechanical properties of the car floor while reducing the weight of the floor. The product has a higher strength-to-weight ratio and maximizes the lightness and high strength of the material properties of poplar and eucalyptus wood themselves, which helps to improve the carrying capacity and endurance of new energy vehicles.
[0045] Further optimizing the scheme, in step 1, the reconstructed surface board 1 is made of a poplar-eucalyptus mixed board formed by mixing and pressing a dispersed poplar veneer and a dispersed eucalyptus veneer;
[0046] The debonded poplar veneer is formed by rolling and debonding the poplar veneer with a linear convex tooth needle roller, so that cracks of uniform length are formed in the direction of the grain of the poplar veneer.
[0047] The eucalyptus veneer is formed by rolling and flaking the poplar veneer with a linear convex tooth needle roller, and forming cracks of uniform length in the direction of the grain of the eucalyptus veneer.
[0048] The poplar-eucalyptus mixed board is obtained by dipping any number of debonded poplar veneers and any number of debonded eucalyptus veneers in glue, drying, assembling and hot pressing to obtain a reconstituted surface board 1.
[0049] Furthermore, the ratio of the number of dispersed poplar veneers to the number of dispersed eucalyptus veneers in the poplar-eucalyptus hybrid board is 1:1.
[0050] Furthermore, in the poplar-eucalyptus mixed board, the poplar veneer and the eucalyptus veneer are arranged at intervals.
[0051] Furthermore, in the poplar-eucalyptus mixed board, the outer surface of the poplar-eucalyptus mixed board is a dispersed poplar veneer.
[0052] Furthermore, the thickness of the poplar-eucalyptus mixed board does not exceed 3 mm.
[0053] To further optimize the solution, in step 2, the wood veneer is selected to be poplar veneer or eucalyptus veneer.
[0054] Further optimizing the scheme, the hybrid composite board includes three wood veneers, and the hybrid composite board is a full poplar, full eucalyptus, or a mixed structure of poplar and eucalyptus;
[0055] The poplar-eucalyptus mixed structure is one of a poplar, eucalyptus, poplar mixed structure or a eucalyptus, poplar, eucalyptus mixed structure.
[0056] According to a further optimization scheme, the thickness of the aramid paper honeycomb material 4 is 3 mm, and the thickness of the film paper 2 is 0.2 mm.
[0057] To further optimize the solution, in step one, the crack thickness matches the thickness of the wood veneer, the crack length is 10-30 mm, the width is 0.1-0.5 mm, the lateral spacing of the cracks is less than 2 mm, and the longitudinal spacing is 5-30 mm.
[0058] To further optimize the solution, the dipping process adopts the pressurized dipping method with the pressure controlled at 3.0-4.0Mpa.
[0059] Further optimization scheme, the aramid paper honeycomb material 4 honeycomb cell side length is 3±0.5mm, honeycomb density is 45±5kg / m 3 ;
[0060] The adhesive paper 2 is made of phenolic resin adhesive paper, and the weight of the adhesive paper base paper is 100-120g / m 2 , the phenolic resin glue impregnation amount is 180%-220%.
[0061] The scheme was further optimized. In step three, the hot pressing temperature was 140°C, the hot pressing time was 1.9 min / mm, and the pressure was set to 0.8-1.2 MPa.
[0062] A lightweight car floor for new energy vehicles is manufactured based on the above-mentioned method for manufacturing a lightweight car floor for new energy vehicles.
[0063] A lightweight car floor for new energy vehicles includes a mixed composite board, which includes a first layer of single board 3, a second layer of single board 5 and a third layer of single board 6. Aramid paper honeycomb material 4 is arranged between the first layer of single board 3 and the second layer of single board 5 and between the second layer of single board 5 and the third layer of single board 6. Film paper 2 is arranged on the top surface of the first layer of single board 3 and the bottom surface of the third layer of single board 6. A reconstructed surface board 1 covers the outside of the film paper 2. The reconstructed surface board 1, the first layer of single board 3, the second layer of single board 5, the third layer of single board 6, the aramid paper honeycomb material 4 and the film paper 2 are combined together by hot pressing to form a lightweight car floor.
[0064] Embodiment 1:
[0065] A method for preparing a lightweight car floor for a new energy vehicle comprises the following steps:
[0066] (1) Preparation of reconstructed surface board 1: Poplar veneer and eucalyptus veneer with a size of 400 mm × 400 mm × 1.7 mm are rolled and loosened by linear convex tooth needle rollers, and cracks of uniform length are formed in the wood veneer along the grain direction, so that the veneer is in a state of loose fiber but not broken. After being polished, it is placed in a dipping barrel and dipped in glue by pressure, with the pressure set to 3.0-4.0 MPa, and the dipping is carried out for 5 minutes, and then dried for 24 hours; after drying, the loosened poplar veneer is used as the reconstructed surface board. On the outer side of the surface plate 1, other prepared poplar veneers and eucalyptus veneers are stacked on the poplar base plate, and the volume ratio of poplar: eucalyptus is 1:1. The poplar veneers and eucalyptus veneers are alternately stacked on the poplar base plate. After stacking, they are laid on the hot pressing plate, first pre-pressed with a pre-pressing pressure of 2MPa for 5min, and then hot pressed with a hot pressing pressure of 1.2MPa, a hot pressing temperature of 140℃, and a hot pressing time of 1.9min / mm; after the hot pressing is completed, cool for 20min and mark the board with a marker.
[0067] (2) Preparation of hybrid composite board: Poplar veneer and eucalyptus veneer are used as basic units, and the veneer is glued on one side with a glue coating amount of 280g / m 2; According to the composite method of poplar-eucalyptus-poplar, the single boards are arranged vertically and crosswise, with loose faces facing loose faces and tight faces facing tight faces. Aramid paper honeycomb material 4 is added between every two single boards for hot pressing to obtain a hollow poplar-eucalyptus staggered structure (P / E) substrate. The hot pressing conditions are: pressure 1.2 MPa, temperature 140°C, time 1.9 min / mm.
[0068] (3) Preparation of hollow recombinant poplar-eucalyptus hybrid composite board: The prepared recombinant surface board 1 is used as the surface board, and the hollow poplar-eucalyptus hybrid composite board with staggered structure is used as the core board, and the single-sided glue is applied with a glue amount of 280g / m 2 , cover the upper and lower surfaces of the reconstructed panel 1, attach a layer of film paper 2 between the two, the film paper 2 is phenolic resin film paper, and perform a secondary hot pressing process; hot pressing conditions: temperature is 140°C, time is 1.9min / mm, among which the hot pressing pressure is set to three different pressure values, which are set to 0.8MPa, 1.0MPa, and 1.2MPa respectively.
[0069] Embodiment 2:
[0070] A method for preparing a lightweight car floor for a new energy vehicle comprises the following steps:
[0071] (1) Preparation of reconstructed surface board 1: Poplar veneer and eucalyptus veneer with a size of 400 mm × 400 mm × 1.7 mm are rolled and loosened by linear convex tooth needle rollers, and cracks of uniform length are formed in the wood veneer along the grain direction, so that the veneer is in a state of loose fiber but not broken. After being polished, it is placed in a dipping barrel and dipped in glue by pressure, with the pressure set to 3.0-4.0 MPa, and the dipping is carried out for 5 minutes, and then dried for 24 hours; after drying, the loosened poplar veneer is used as the reconstructed surface board. On the outer side of the surface plate 1, other prepared poplar veneers and eucalyptus veneers are stacked on the poplar base plate, and the volume ratio of poplar: eucalyptus is 1:1. The poplar veneers and eucalyptus veneers are alternately stacked on the poplar base plate. After stacking, they are laid on the hot pressing plate, first pre-pressed with a pre-pressing pressure of 2MPa for 5min, and then hot pressed with a hot pressing pressure of 1.2MPa, a hot pressing temperature of 140℃, and a hot pressing time of 1.9min / mm; after the hot pressing is completed, cool for 20min and mark the board with a marker.
[0072] (2) Preparation of hybrid composite board: Poplar veneer and eucalyptus veneer are used as basic units, and the veneer is glued on one side with a glue coating amount of 280g / m 2 ; According to the composite method of eucalyptus-poplar-eucalyptus, the single boards are arranged vertically and crosswise, with loose faces facing loose faces and tight faces facing tight faces. Aramid paper honeycomb material 4 is added between every two single boards for hot pressing to obtain a hollow eucalyptus-poplar staggered structure (E / P) substrate. The hot pressing conditions are: pressure 1.2 MPa, temperature 140°C, and time 1.9 min / mm.
[0073] (3) Preparation of hollow recombinant poplar-eucalyptus hybrid composite board: The prepared recombinant poplar-eucalyptus board is used as the surface board, and the hollow eucalyptus-poplar interlaced structure substrate is used as the core board. The single-sided glue is applied with a glue amount of 280g / m 2 , cover the upper and lower surfaces with the recombinant poplar eucalyptus surface board, attach a layer of phenolic resin film paper between the two, and carry out a secondary hot pressing process; hot pressing conditions: temperature is 140℃, time is 1.9min / mm, among which the hot pressing pressure is set to three different pressure values, which are set to 0.8MPa, 1.0MPa, and 1.2MPa respectively.
[0074] Embodiment 3:
[0075] A method for preparing a lightweight car floor for a new energy vehicle comprises the following steps:
[0076] (1) Preparation of reconstructed surface board 1: Poplar veneer and eucalyptus veneer with a size of 400 mm × 400 mm × 1.7 mm are rolled and loosened by linear convex tooth needle rollers, and cracks of uniform length are formed in the wood veneer along the grain direction, so that the veneer is in a state of loose fiber but not broken. After being polished, it is placed in a dipping barrel and dipped in glue by pressure, with the pressure set to 3.0-4.0 MPa, and the dipping is carried out for 5 minutes, and then dried for 24 hours; after drying, the loosened poplar veneer is used as the reconstructed surface board. On the outer side of the surface plate 1, other prepared poplar veneers and eucalyptus veneers are stacked on the poplar base plate, and the volume ratio of poplar: eucalyptus is 1:1. The poplar veneers and eucalyptus veneers are alternately stacked on the poplar base plate. After stacking, they are laid on the hot pressing plate, first pre-pressed with a pre-pressing pressure of 2MPa for 5min, and then hot pressed with a hot pressing pressure of 1.2MPa, a hot pressing temperature of 140℃, and a hot pressing time of 1.9min / mm; after the hot pressing is completed, cool for 20min and mark the board with a marker.
[0077] (2) Preparation of hybrid composite board: Poplar veneer and eucalyptus veneer are used as basic units, and the veneer is glued on one side with a glue coating amount of 280g / m 2 ; Eucalyptus-eucalyptus-eucalyptus composite combination, single board cross vertical arrangement, loose surface to loose surface, tight surface to tight surface, add aramid paper honeycomb material 4 between every two single boards for hot pressing, to obtain a hollow poplar-eucalyptus staggered structure (E / E) substrate, hot pressing conditions: pressure 1.2MPa, temperature 140℃, time 1.9min / mm.
[0078] (3) Preparation of hollow recombinant poplar-eucalyptus hybrid composite board: The prepared recombinant surface board 1 is used as the surface board, and the hollow poplar-eucalyptus hybrid composite board with staggered structure is used as the core board, and the single-sided glue is applied with a glue amount of 280g / m 2, cover the upper and lower surfaces of the reconstructed panel 1, attach a layer of film paper 2 between the two, the film paper 2 is phenolic resin film paper, and perform a secondary hot pressing process; hot pressing conditions: temperature is 140°C, time is 1.9min / mm, among which the hot pressing pressure is set to three different pressure values, which are set to 0.8MPa, 1.0MPa, and 1.2MPa respectively.
[0079] Embodiment 4:
[0080] A method for preparing a lightweight car floor for a new energy vehicle comprises the following steps:
[0081] (1) Preparation of reconstructed surface board 1: Poplar veneer and eucalyptus veneer with a size of 400 mm × 400 mm × 1.7 mm are rolled and loosened by linear convex tooth needle rollers, and cracks of uniform length are formed in the wood veneer along the grain direction, so that the veneer is in a state of loose fiber but not broken. After being polished, it is placed in a dipping barrel and dipped in glue by pressure, with the pressure set to 3.0-4.0 MPa, and the dipping is carried out for 5 minutes, and then dried for 24 hours; after drying, the loosened poplar veneer is used as the reconstructed surface board. On the outer side of the surface plate 1, other prepared poplar veneers and eucalyptus veneers are stacked on the poplar base plate, and the volume ratio of poplar: eucalyptus is 1:1. The poplar veneers and eucalyptus veneers are alternately stacked on the poplar base plate. After stacking, they are laid on the hot pressing plate, first pre-pressed with a pre-pressing pressure of 2MPa for 5min, and then hot pressed with a hot pressing pressure of 1.2MPa, a hot pressing temperature of 140℃, and a hot pressing time of 1.9min / mm; after the hot pressing is completed, cool for 20min and mark the board with a marker.
[0082] (2) Preparation of hybrid composite board: Poplar veneer and eucalyptus veneer are used as basic units, and the veneer is glued on one side with a glue coating amount of 280g / m 2 ; The single boards are arranged vertically and crosswise in a composite manner of poplar-poplar-poplar, with loose faces facing loose faces and tight faces facing tight faces. Aramid paper honeycomb material 4 is added between every two single boards for hot pressing to obtain a hollow eucalyptus-poplar staggered structure (P / P) substrate. The hot pressing conditions are: pressure 1.2 MPa, temperature 140°C, and time 1.9 min / mm.
[0083] (3) Preparation of hollow recombinant poplar-eucalyptus hybrid composite board: The prepared recombinant poplar-eucalyptus board is used as the surface board, and the hollow eucalyptus-poplar interlaced structure substrate is used as the core board. The single-sided glue is applied with a glue amount of 280g / m 2 , cover the upper and lower surfaces with the recombinant poplar eucalyptus surface board, attach a layer of phenolic resin film paper between the two, and carry out a secondary hot pressing process; hot pressing conditions: temperature is 140℃, time is 1.9min / mm, among which the hot pressing pressure is set to three different pressure values, which are set to 0.8MPa, 1.0MPa, and 1.2MPa respectively.
[0084] The recombinant poplar-eucalyptus hybrid composite board obtained by treatment in Example 1-4 was measured according to GB / T17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", and the density (ρ), moisture content (H), 24h water absorption (WA), 24h water absorption thickness expansion rate (TS), static bending strength (MOR), elastic modulus (MOE) and bonding strength (BS) indicators of the recombinant poplar-eucalyptus hybrid composite board were mainly tested. Each group of performance was measured 5 times, and the test results and physical and mechanical properties are shown in Table 1 below.
[0085] Table 1 Performance results of recombinant poplar-eucalyptus hybrid composite board
[0086]
[0087] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0088] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for manufacturing a lightweight car floor for a new energy vehicle, characterized in that: The steps include: Step 1: Making a reorganization table (1); Step 2: Take a specified number of wood veneers, apply glue to the veneers, set an aramid paper honeycomb material (4) between two adjacent wood veneers, and fix them by hot pressing to obtain a hybrid composite board; Step 3: placing adhesive film paper (2) on the upper and lower surfaces of the hybrid composite board; Step 4: Cover the reconstructed surface plate (1) on the upper and lower surfaces of the hybrid composite plate on which the adhesive film paper (2) is provided, and then fix and shape them by hot pressing.
2. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 1, characterized in that: In the step 1, the reconstructed surface board (1) is made of a poplar-eucalyptus mixed board formed by mixing and pressing a debonded poplar veneer and a debonded eucalyptus veneer; The debonded poplar veneer is formed by rolling and debonding the poplar veneer with a linear convex tooth needle roller, so that cracks of uniform length are formed in the direction of the grain of the poplar veneer. The debonded eucalyptus veneer is formed by rolling and debonding a poplar veneer with a linear convex tooth needle roller, so that cracks of uniform length are formed in the eucalyptus veneer in the direction of the grain; The poplar-eucalyptus mixed board is obtained by subjecting any number of debonded poplar veneers and any number of debonded eucalyptus veneers to the process of gluing, drying, assembling and hot pressing to obtain the reconstituted surface board (1).
3. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 1, characterized in that: In the step 2, the wood veneer is selected to be a poplar veneer or a eucalyptus veneer.
4. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 3, characterized in that: The hybrid composite board comprises three wood veneers, and the hybrid composite board is a structure of all poplar, all eucalyptus, or a mixed structure of poplar and eucalyptus; The poplar-eucalyptus mixed structure is one of poplar, eucalyptus, poplar mixed structure or eucalyptus, poplar, eucalyptus mixed structure.
5. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 1, characterized in that: The thickness of the aramid paper honeycomb material (4) is 3 mm, and the thickness of the adhesive film paper (2) is 0.2 mm.
6. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 2, characterized in that: The crack thickness of the debonded poplar veneer matches the thickness of the debonded poplar veneer, and the crack thickness of the debonded eucalyptus veneer matches the thickness of the debonded eucalyptus veneer; The length of the crack is 10-30 mm, the width is 0.1-0.5 mm, the lateral spacing of the crack is less than 2 mm, and the longitudinal spacing is 5-30 mm.
7. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 1, characterized in that: The dipping process is carried out by a pressurized dipping method, and the pressure is controlled to be 3.0-4.0 MPa.
8. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 5, characterized in that: The aramid paper honeycomb material (4) has a honeycomb cell side length of 3±0.5 mm and a honeycomb density of 45±5 kg / m 3 ; The adhesive paper (2) is made of phenolic resin adhesive paper, and the weight of the adhesive paper base paper is 100-120 g / m 2 , the phenolic resin glue impregnation amount is 180%-220%.
9. The method for manufacturing a lightweight car floor for a new energy vehicle according to claim 1, characterized in that: In the step three, the hot pressing temperature is 140° C., the hot pressing time is 1.9 min / mm, and the pressure is set to 0.8-1.2 MPa.
10. A lightweight car floor for a new energy vehicle, manufactured based on the manufacturing method of a lightweight car floor for a new energy vehicle according to any one of claims 1-9.
Citation Information
Patent Citations
Veneer pressurization gumming enhancement type composite container floor and manufacturing method thereof
CN101214667A
Recombination wood and manufacturing method thereof
CN101357470A
Composite panel for green building
CN105986639A
Wood veneer treatment method and reconstituted wood
CN106426430A
Composite bed board for motorhome
CN108688549A