All-olefin composite membrane as well as preparation method and application thereof

By adopting the design of modified CPP film, the food safety, environmental protection and strength of the existing tote bag composite film materials is solved, and the all-olefin composite film with high transparency, high strength and good flexibility is achieved, which improves the tote bag's Performance and environmental protection.

CN119058199AActive Publication Date: 2024-12-03HUANGSHAN NOVEL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411173051.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The composite membrane materials of existing transparent handbags have problems such as solvent residues, resulting in food safety problems, unenvironmental protection, low transparency, insufficient strength of the handbore holes, and easy to break.

Method used

A full olefin composite film consisting of BOPP film, ink layer, extruded resin layer and modified CPP film is used. The modified CPP film consists of extruded layer, intermediate layer and heat sealing layer, and random copolymerized polypropylene and ethylene are used— Materials such as octene elastomer, metallocene copolymer polypropylene, etc. form a composite film with high transparency, high strength and good flexibility through coextrusion casting and the design of the bonding layer.

Benefits of technology

It realizes a full olefin composite film with high transparency, high strength and good flexibility without adhesives, improves the handle strength, peel strength and heat seal strength of the hand bag, and enhances environmental protection and recycling value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119058199A_ABST
    Figure CN119058199A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of packaging, and particularly relates to a total-olefin composite film as well as a preparation method and application thereof. The composite film is composed of a BOPP film, an ink layer, an extrusion resin layer and a modified CPP film which are connected in sequence. The modified CPP film is composed of an extrusion layer, a middle layer and a heat sealing layer. The extrusion resin layer is composed of a first bonding layer and a second bonding layer, the first bonding layer is connected with the ink layer, and the second bonding layer is connected with the extrusion layer. The all-olefin composite film does not use an adhesive, can be recycled, has high transparency and high strength, and is not easy to break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging, in particular to an all-olefin composite film and a preparation method and application thereof. Background Art

[0002] Transparent handbags are widely used in product promotion packaging. This type of outer bag is generally made of PET / PE or BOPP / CPP composite film. This type of packaging is convenient for consumers to purchase in small quantities, and it is a complete package with a hand hole for easy transportation. This type of outer bag requires: good transparency to clearly display the packaged product inside; good hand hole fastness to ensure that it will not break after repeated transportation by consumers; the composite film should be soft and will not hurt the hands of the transporter; the peeling and sealing strength should ensure that it cannot be damaged by the weight of the contents.

[0003] At present, this type of handbag has the following problems:

[0004] 1) The composite film material of PET / PE is used, and adhesives are used, which will leave solvent residues. Not only does it cause food safety issues, but the purity of the final handbag is generally around 97%, which cannot be 100% recycled and reused, and is not environmentally friendly;

[0005] 2) The contents cannot be clearly displayed and the transparency is average;

[0006] 2) The composite film of BOPP / CPP material is too brittle, the handle strength is low and easy to break; the peeling and heat sealing strength is low, and it is easy to delaminate and break when pulling. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a self-supporting bag that can be opened by straight-line tearing and a production process thereof. The all-olefin composite film does not use adhesives, is recyclable, and has the advantages of high transparency, high strength, and is not easy to break.

[0008] In order to achieve one of the purposes of the present invention, the present invention adopts the following technical solutions:

[0009] An all-olefin composite film, which consists of a BOPP film, an ink layer, an extruded resin layer and a modified CPP film connected in sequence, wherein the modified CPP film consists of an extruded layer, an intermediate layer and a heat-sealing layer; the extruded layer consists of 80-90 parts by weight of random copolymerized polypropylene and 10-20 parts by weight of ethylene-octene elastomer, the intermediate layer consists of 80-90 parts by weight of random copolymerized polypropylene and 10-20 parts by weight of propylene-based elastomer, the heat-sealing layer consists of 60-70 parts by weight of metallocene copolymerized polypropylene, 25-35 parts by weight of metallocene polyethylene, 1.5-2.5 parts by weight of a slip agent and 2.5-3.5 parts by weight of a silicon oxide opening agent; the extruded resin layer consists of a first adhesive layer and a second adhesive layer, the first adhesive layer is connected to the ink layer, and the second adhesive layer is connected to the extruded layer.

[0010] Preferably, the first adhesive layer is composed of 60-70 parts by mass of metallocene vinyl plastomer and 30-40 parts by mass of ethylene-methyl methacrylate copolymer; the second adhesive layer is composed of 100 parts by mass of metallocene vinyl plastomer; the ink used in the ink layer is GC single lipid environmentally friendly ink produced by Sony Ink Company.

[0011] Preferably, the brand of the metallocene vinyl plastomer is PT1450 produced by The Dow Chemical Company; the brand of the ethylene-methyl methacrylate copolymer is WH401-F produced by Sumitomo Corporation of Japan.

[0012] Preferably, the brand of random copolymer polypropylene is RD368CF produced by Borouge; the brand of ethylene-octene elastomer is ENGAGE8200 produced by DowDuPont; the brand of propylene-based elastomer is 3980 produced by Exxon; the brand of metallocene copolymer polypropylene is WFX4TA produced by Japan PP; the brand of metallocene polyethylene is SP0540 produced by Mitsui; the brand of slip agent is SLIP-7 produced by Aaron; the brand of silica opening agent is AB-20LD produced by Aaron.

[0013] Preferably, the extruded layer is composed of 85 parts by mass of random copolymer polypropylene and 15 parts by mass of ethylene-octene elastomer, the intermediate layer is composed of 85 parts by mass of random copolymer polypropylene and 15 parts by mass of propylene-based elastomer, and the heat-sealing layer is composed of 65 parts by mass of metallocene copolymer polypropylene, 30 parts by mass of metallocene polyethylene, 2 parts by mass of a lubricant and 3 parts by mass of an opening agent.

[0014] Preferably, the thickness of the BOPP film is 18-38um; the thickness of the ink layer is 1-2um; the thickness of the extruded resin layer is 13-20um; and the thickness of the modified CPP film is 30-50um.

[0015] Preferably, the thickness ratio of the first adhesive layer to the second adhesive layer is 1:1.

[0016] Preferably, the BOPP film is made by printing a BOPP film.

[0017] In order to achieve the second object of the present invention, the present invention provides a method for preparing an all-olefin composite film, comprising the following steps:

[0018] S1. Preparing a modified CPP film: Weighing the extrusion layer resin, the middle layer resin and the heat sealing layer resin in respective weight parts, and sequentially subjecting the extrusion layer resin to co-extrusion casting, cooling and shaping, thickness measurement, slitting and winding to obtain a modified CPP film;

[0019] S2. Preparation of extruded resin layer: Weigh the first adhesive layer resin and the second adhesive layer resin in parts by mass respectively, and pass them through co-extrusion coating and lamination of two extruders and one die head in sequence. When the coating comes out of the die, immediately bond the first adhesive layer to the side of the BOPP film printed with the ink layer, and bond the second adhesive layer to the modified CPP film, and use auxiliary pressing rollers and quenching rollers to roll up after bonding and cooling to obtain an extruded composite film.

[0020] In order to achieve the third purpose of the present invention, the present invention provides an application of an all-olefin composite film, wherein the composite film is used to prepare a transparent handbag.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The composite film of the present invention is a full olefin film and does not use adhesives, which is more conducive to the recycling and granulation of composite film waste after consumption. The modified CPP film is designed with a high transparency and high flexibility formula and an optimized production process.

[0023] 2) The all-olefin composite film structure of the present invention improves the handle strength, increases the transparency of the bag body, enhances the flexibility, and improves the peel strength and heat sealing strength.

[0024] 3) The modified CPP film of the present invention adopts copolymerized polypropylene and metallocene polypropylene resin, and adds elastomeric resin for toughening modification;

[0025] Among them, the extrusion layer uses random copolymer polypropylene and ethylene-octene elastomer blended together. Ethylene-octene elastomer has good compatibility with polypropylene and polyethylene, which can improve the bonding strength with the extruded resin, that is, the peel strength. The middle layer uses random copolymer polypropylene and propylene-based elastomer blended together. Propylene-based elastomer has good compatibility with polypropylene and can form flexible segments to improve the flexibility of the modified CPP film. The heat-sealing layer uses metallocene copolymer polypropylene and cast-grade metallocene polyethylene blended together, and adds a lubricant and an opening agent. The metallocene polyethylene resin has low-temperature heat sealing properties, high elongation, good flexibility after heat sealing, and the heat-sealed area is not easy to burst. The opening agent is an inorganically filled opening agent, which allows a tiny air layer to be formed between the films to avoid vacuum adhesion of the films. The lubricant is an erucic acid amide filled lubricant, which has mobility and can migrate to the heat-sealing surface of the film after film formation, that is, the inner surface of the bag, which helps to open the bag and fill the contents smoothly.

[0026] 4) The extruded resin in the present invention uses two layers of adhesive layers to coextrude into an adhesive film. The metallocene vinyl plastomer used has good compatibility with polypropylene and polyethylene, and can produce good bonding strength with the area without ink on the BOPP film. The ethylene segment in the ethylene-methyl methacrylate copolymer used has good compatibility with the metallocene vinyl plastomer, and the methyl methacrylate segment has good adhesion to the polyurethane ink layer. The adhesive layer connected to the modified CPP film is a pure metallocene vinyl plastomer resin, which has good adhesion to the extruded layer of the modified CPP film, thereby obtaining a high-peel composite film.

[0027] 5) Different from conventional CPP films, the modified CPP film of the present invention does not require polarized corona treatment on the film surface during production, and its extrusion bonding is based on the compatibility mechanism of the resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a structural diagram of the present invention;

[0029] Figure 2 It is a schematic diagram of the process flow of the modified CPP film of the present invention.

[0030] The meanings of the symbols in the figure are as follows:

[0031] 1-BOPP film, 2-ink layer, 3-extruded resin layer, 4-modified CPP film. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] An all-olefin composite film, the composite film is composed of a BOPP film 1, an ink layer 2, an extruded resin layer 3 and a modified CPP film 4 connected in sequence, the modified CPP film 4 is composed of an extruded layer, an intermediate layer and a heat-sealing layer; the extruded resin layer 3 is composed of a first adhesive layer and a second adhesive layer. The thickness of the BOPP film 1 is 18um, the thickness of the extruded resin layer 3 is 20um, and the thickness of the modified CPP film 4 is 40um.

[0035] Among them, the first adhesive layer is connected to the ink layer 2, and the second adhesive layer is connected to the extruded layer; the extruded layer is composed of 80 parts by mass of random copolymer polypropylene and 20 parts by mass of ethylene-octene elastomer, the middle layer is composed of 90 parts by mass of random copolymer polypropylene and 10 parts by mass of propylene-based elastomer, and the heat-sealing layer is composed of 60 parts by mass of metallocene copolymer polypropylene, 35 parts by mass of metallocene polyethylene, 2.5 parts by mass of lubricant and 2.5 parts by mass of silica opening agent.

[0036] The first adhesive layer is composed of 60 parts by mass of metallocene vinyl plastomer and 40 parts by mass of ethylene-methyl methacrylate copolymer; the second adhesive layer is composed of 100 parts by mass of metallocene vinyl plastomer; the ink used in ink layer 2 is GC single lipid environmentally friendly ink produced by Sony Ink Company.

[0037] A method for preparing an all-olefin composite film comprises the following steps:

[0038] S1, preparing modified CPP film 4: respectively weighing the mass parts of extrusion layer resin, intermediate layer resin and heat sealing layer resin, and sequentially performing co-extrusion casting, cooling and shaping, thickness measurement, slitting and winding to obtain modified CPP film 4, the process flow is as follows: Figure 2 As shown;

[0039] S2. Preparation of extruded resin layer 3: Weigh the first adhesive layer resin and the second adhesive layer resin in parts by mass respectively, and pass them through co-extrusion coating of two extruders and one die head in sequence. When the coating comes out of the die, immediately bond the first adhesive layer to the side of the BOPP film 1 printed with the ink layer 2, and bond the second adhesive layer to the modified CPP film 4, and use auxiliary lamination rollers and quenching rollers to roll up after bonding and cooling to obtain the extruded composite film 1.

[0040] Example 2

[0041] An all-olefin composite film, the composite film is composed of a BOPP film 1, an ink layer 2, an extruded resin layer 3 and a modified CPP film 4 connected in sequence, the modified CPP film 4 is composed of an extruded layer, an intermediate layer and a heat-sealing layer; the extruded resin layer 3 is composed of a first adhesive layer and a second adhesive layer. The thickness of the BOPP film 1 is 28um, the thickness of the extruded resin layer 3 is 15um, and the thickness of the modified CPP film 4 is 35um.

[0042] Among them, the first adhesive layer is connected to the ink layer 2, and the second adhesive layer is connected to the extruded layer; the extruded layer is composed of 85 parts by mass of random copolymer polypropylene and 15 parts by mass of ethylene-octene elastomer, the middle layer is composed of 85 parts by mass of random copolymer polypropylene and 15 parts by mass of propylene-based elastomer, and the heat-sealing layer is composed of 65 parts by mass of metallocene copolymer polypropylene, 30 parts by mass of metallocene polyethylene, 2 parts by mass of lubricant and 3 parts by mass of silica opening agent.

[0043] The first adhesive layer is composed of 70 parts by mass of metallocene vinyl plastomer and 30 parts by mass of ethylene-methyl methacrylate copolymer; the second adhesive layer is composed of 100 parts by mass of metallocene vinyl plastomer; the ink used in ink layer 2 is GC single lipid environmentally friendly ink produced by Sony Ink Company.

[0044] A method for preparing an all-olefin composite film comprises the following steps:

[0045] S1, preparing modified CPP film 4: respectively weighing the mass parts of extrusion layer resin, intermediate layer resin and heat sealing layer resin, and sequentially subjecting to co-extrusion casting, cooling and shaping, thickness measurement, corona treatment, slitting and winding to obtain modified CPP film 4. The process flow is as follows: Figure 2 As shown;

[0046] S2. Preparation of extruded resin layer 3: Weigh the first adhesive layer resin and the second adhesive layer resin in parts by mass respectively, and pass them through co-extrusion coating of two extruders and one die head in sequence. When the coating comes out of the die, immediately bond the first adhesive layer to the side of the BOPP film 1 printed with the ink layer 2, and bond the second adhesive layer to the modified CPP film 4, and use auxiliary lamination rollers and quenching rollers to roll up after bonding and cooling to obtain the extruded composite film 2.

[0047] Example 3

[0048] A full olefin composite film, which is composed of a BOPP film 1, an ink layer 2, an extruded resin layer 3 and a modified CPP film 4 connected in sequence. The modified CPP film 4 is composed of an extruded layer, an intermediate layer and a heat-sealing layer; the extruded resin layer 3 is composed of a first adhesive layer and a second adhesive layer.

[0049] The first adhesive layer is connected to the ink layer 2, and the second adhesive layer is connected to the extruded layer; the extruded layer is composed of 90 parts by mass of random copolymerized polypropylene and 10 parts by mass of ethylene-octene elastomer, the middle layer is composed of 80 parts by mass of random copolymerized polypropylene and 20 parts by mass of propylene-based elastomer, and the heat-sealing layer is composed of 70 parts by mass of metallocene copolymerized polypropylene, 25 parts by mass of metallocene polyethylene, 1.5 parts by mass of slip agent and 3.5 parts by mass of silicon oxide opening agent. The thickness of the BOPP film 1 is 38um, the thickness of the extruded resin layer 3 is 13um, and the thickness of the modified CPP film 4 is 30um.

[0050] The first adhesive layer is composed of 65 parts by mass of metallocene vinyl plastomer and 35 parts by mass of ethylene-methyl methacrylate copolymer; the second adhesive layer is composed of 100 parts by mass of metallocene vinyl plastomer; the ink used in ink layer 2 is GC single lipid environmentally friendly ink produced by Sony Ink Company.

[0051] A method for preparing an all-olefin composite film comprises the following steps:

[0052] S1, preparing modified CPP film 4: respectively weighing the mass parts of extrusion layer resin, intermediate layer resin and heat sealing layer resin, and sequentially subjecting to co-extrusion casting, cooling and shaping, thickness measurement, corona treatment, slitting and winding to obtain modified CPP film 4. The process flow is as follows: Figure 2 As shown;

[0053] S2. Preparation of extruded resin layer 3: Weigh the first adhesive layer resin and the second adhesive layer resin in parts by mass respectively, and pass them through co-extrusion coating of two extruders and one die head in sequence. When the coating comes out of the die, immediately bond the first adhesive layer to the side of the BOPP film 1 printed with the ink layer 2, and bond the second adhesive layer to the modified CPP film 4, and use auxiliary lamination rollers and quenching rollers to roll up after bonding and cooling to obtain the extruded composite film 3.

[0054] The formula and particle performance parameters of the modified CPP film in Examples 1 to 3 are shown in Tables 1-2 below, and the casting process parameters of the modified CPP film are shown in Table 3 below:

[0055] Table 1 is the modified CPP film formula

[0056]

[0057] Table 2 Particle information table

[0058]

[0059] Table 3 Casting process parameters of modified CPP film

[0060]

[0061]

[0062] Comparative Example 1

[0063] The composite film 4 is composed of a BOPP film with a thickness of 28 μm and a CPP film with a thickness of 50 μm.

[0064] Comparative Example 2

[0065] The composite film 5 is composed of a PET film with a thickness of 12 μm and a PE film with a thickness of 65 μm.

[0066] The composite film 2 prepared in Example 2 and the composite films 4-5 in Comparative Examples 1-2 were prepared into handbags, and the performance of the handbags was tested. The results are shown in Table 4 below:

[0067] Table 4 Test results of composite film and bag making

[0068]

[0069]

[0070] It can be seen from Table 4 that the composite film prepared in Example 2 has the largest tensile force, and the peel strength and heat sealing strength are significantly higher than those of Comparative Example 1, and the haze is the lowest, the contents are displayed most clearly, and there is no breakage in the handle test. The material is made of all-olefin composites, and the post-consumer products can be recycled at a high value and can be recycled, which meets environmental protection requirements.

Claims

1. An all-olefin composite film, characterized in that: The composite film is composed of a BOPP film (1), an ink layer (2), an extruded resin layer (3) and a modified CPP film (4) which are connected in sequence, wherein the modified CPP film (4) is composed of an extruded layer, an intermediate layer and a heat-sealing layer; the extruded layer is composed of 80-90 parts by weight of random copolymerized polypropylene and 10-20 parts by weight of ethylene-octene elastomer, the intermediate layer is composed of 80-90 parts by weight of random copolymerized polypropylene and 10-20 parts by weight of propylene-based elastomer, the heat-sealing layer is composed of 60-70 parts by weight of metallocene copolymerized polypropylene, 25-35 parts by weight of metallocene polyethylene, 1.5-2.5 parts by weight of a slip agent and 2.5-3.5 parts by weight of a silicon oxide opening agent; the extruded resin layer (3) is composed of a first adhesive layer and a second adhesive layer, wherein the first adhesive layer is connected to the ink layer (2) and the second adhesive layer is connected to the extruded layer.

2. The all-olefin composite film according to claim 1, characterized in that: The first adhesive layer is composed of 60-70 parts by weight of metallocene vinyl plastomer and 30-40 parts by weight of ethylene-methyl methacrylate copolymer; the second adhesive layer is composed of 100 parts by weight of metallocene vinyl plastomer; the ink used in the ink layer (2) is GC single lipid environmentally friendly ink produced by Sony Ink Company.

3. An all-olefin composite film according to claim 2, characterized in that: The brand of the metallocene vinyl plastomer is PT1450 produced by Dow Chemical Company; the brand of the ethylene-methyl methacrylate copolymer is WH401-F produced by Sumitomo Corporation of Japan.

4. The all-olefin composite film according to claim 1, characterized in that: The brand of the random copolymer polypropylene is RD368CF produced by Borouge; the brand of the ethylene-octene elastomer is ENGAGE8200 produced by DowDuPont; the brand of the propylene-based elastomer is 3980 produced by Exxon; the brand of the metallocene copolymer polypropylene is WFX4TA produced by Japan PP; the brand of the metallocene polyethylene is SP0540 produced by Mitsui; the brand of the slip agent is SLIP-7 produced by Aaron; and the brand of the silica opening agent is AB-20LD produced by Aaron.

5. The all-olefin composite film according to claim 1, characterized in that: The extruded layer is composed of 85 parts by mass of random copolymerized polypropylene and 15 parts by mass of ethylene-octene elastomer, the intermediate layer is composed of 85 parts by mass of random copolymerized polypropylene and 15 parts by mass of propylene-based elastomer, and the heat-sealing layer is composed of 65 parts by mass of metallocene copolymerized polypropylene, 30 parts by mass of metallocene polyethylene, 2 parts by mass of a slip agent and 3 parts by mass of an anti-blocking agent.

6. The all-olefin composite film according to claim 1, characterized in that: The thickness of the BOPP film (1) is 18-38 um; the thickness of the ink layer (2) is 1-2 um; the thickness of the extruded resin layer (3) is 13-20 um; and the thickness of the modified CPP film (4) is 30-50 um.

7. The all-olefin composite film according to claim 1, characterized in that: The thickness ratio of the first adhesive layer to the second adhesive layer is 1:

1.

8. The all-olefin composite film according to claim 1, characterized in that: The BOPP film (1) is made by printing a BOPP film.

9. A method for preparing an all-olefin composite film according to any one of claims 1 to 8, characterized in that: The steps include: S1. Preparing a modified CPP film (4): Weighing respective weight portions of an extrusion layer resin, an intermediate layer resin and a heat-sealing layer resin, and sequentially subjecting the co-extrusion casting, cooling and shaping, thickness measurement, slitting and winding to obtain a modified CPP film (4); S2. Preparation of extruded resin layer (3): Weigh the first adhesive layer resin and the second adhesive layer resin in respective mass parts, and sequentially pass them through co-extrusion coating of two extruders and one die head. When the coating exits the die, immediately bond the first adhesive layer to the side of the BOPP film (1) printed with the ink layer (2), and bond the second adhesive layer to the modified CPP film (4), and use auxiliary lamination rollers and quenching rollers to roll up after bonding and cooling to obtain an extruded composite film.

10. An application of the all-olefin composite film according to any one of claims 1 to 8, characterized in that: The composite film is used for preparing a transparent handbag.

Citation Information

Patent Citations

  • Tear-resistant polyethylene film, composite membrane and preparation method thereof

    CN107323053A

  • Olefins protective film

    CN107722863A

  • Flexible package modified CPP film and production method thereof

    CN115139615A

  • Medicinal composite membrane as well as preparation method and application thereof

    CN117227291A

  • High-transparency antistatic high-toughness polypropylene composite film and preparation process thereof

    CN117774473A