Preparation method of surface-passivated Prussian blue analogue and energy storage device

A surface-passivated Prussian blue analogue is prepared via a coprecipitation method, addressing air stability and cycle stability issues in sodium-ion batteries, enhancing their suitability for industrial use.

CN119059533AActive Publication Date: 2024-12-03WENZHOU NATECH NEW ENERGY TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411549934.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-12-03
Estimated Expiration
2044-11-01

AI Technical Summary

Technical Problem

Current sodium-ion batteries face challenges in air stability and electrode surface loading, which hinder their industrial application due to high costs and low energy and power density.

Method used

A surface-passivated Prussian blue analogue is prepared through a coprecipitation method using chelating agents, ferrous and zinc salts, and ascorbic acid, followed by centrifugal washing and vacuum freeze-drying, enhancing air stability and cycle stability.

Benefits of technology

The method results in a Prussian blue analogue with improved air stability and cycle stability, suitable for high-surface-loading electrodes, facilitating industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059533A_ABST
    Figure CN119059533A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion battery positive electrode materials, and particularly relates to a preparation method of a surface-passivated Prussian blue analogue and an energy storage device. A simple coprecipitation method is adopted, and surface passivation metal ions are introduced into the Prussian blue analogue to regulate and control the surface appearance. The surface-passivated iron-based prussian blue analogue shows good air stability, and shows excellent electrochemical performance under high surface load at the same time. The technological process is simple and convenient, the cost is low, and the designed high-surface-load electrode material conforms to actual industrial production in a sodium-ion battery energy storage system and has high commercial practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a preparation method of a surface passivated Prussian blue analogue and an energy storage device thereof. Background Art

[0002] The growing market demand for portable electronic products, grid-level energy storage and electric vehicles has driven the development of rechargeable batteries. Compared with lithium-ion batteries, sodium-ion batteries have the advantages of abundant sodium resources and low prices, which are very suitable for low-cost energy storage applications. The current mainstream sodium cathode materials are mainly polyanion compounds, Prussian blue and layered transition metal oxides. Prussian blue analogs have gradually become a hot topic of research in academia and industry due to their unique open-frame structure, abundant sodium storage sites and large ion migration channels. However, in order to reduce the cost of raw material protection during the industrialization of sodium-ion batteries and to increase the energy density and power density of the battery, it is necessary to improve the air stability and electrode surface loading of the material to realize the practical application of high-energy batteries. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for preparing a surface-passivated Prussian blue analogue. By surface-passivating the Prussian blue analogue, the air stability of the Prussian blue analogue is improved, and at the same time, the cycle stability of the high-surface-loaded positive electrode material is improved.

[0004] A first aspect of the present invention provides a method for preparing a surface-passivated and air-stable Prussian blue analogue, comprising the following steps: S1, dissolve a certain amount of chelating agent in 100 mL of deionized water, then add ferrous salt, zinc salt and ascorbic acid, stir to dissolve, and record it as solution A.

[0005] S2, dissolve a certain amount of sodium ferrocyanide in 100 mL of deionized water, recorded as solution B.

[0006] S3, slowly dripping the solution prepared in steps S1 and S2 into solution C containing 50 mL of deionized water at a certain dripping rate, and stirring for a period of time at a certain temperature and stirring speed.

[0007] S4, allowing the mixed solution of step S3 to stand and age for a period of time at a certain temperature.

[0008] S5, after the reaction is completed, the obtained product is centrifugally washed with deionized water and anhydrous ethanol for multiple times, and vacuum freeze-dried for a period of time to finally obtain a blue powder, which is a surface-passivated Prussian blue analogue.

[0009] The chelating agent in step S1 is one or more of citric acid, sodium citrate, disodium ethylenediaminetetraacetic acid and sodium pyrophosphate, and preferably the chelating agent is sodium citrate.

[0010] The zinc salt in step S1 is one or more of zinc sulfate, zinc chloride, zinc phosphate, and zinc nitrate, and preferably the zinc salt is zinc sulfate.

[0011] The ferrous salt in step S1 is one or more of ferrous sulfate, ferrous chloride, ferrous nitrate, and ferrous acetate, and preferably the ferrous salt is ferrous sulfate.

[0012] Preferably, the concentration of the chelating agent is 0-2 mol L -1 , the concentration of zinc salt is 0-0.1 mol L -1 , the concentration of ascorbic acid is 0-0.2 mol L -1 The concentration of ferrous salt is 0-0.5 mol L -1 More preferably, the concentration of the chelating agent is 1.8 mol L -1 , the concentration of zinc salt is 0.045 mol L -1 , the concentration of ascorbic acid was 0.085 mol L -1 The concentration of ferrous salt is 0.405 mol L -1 .

[0013] Preferably, the concentration of sodium ferrocyanide is 0-0.5 mol L -1 More preferably, the concentration of sodium ferrocyanide is 0.45 mol L -1 .

[0014] Preferably, the dripping rate in step S3 is 10 mL h -1 -20 mL h -1 , the stirring speed is 400-500 rmp, the stirring time is 0.5-3 h, the stirring temperature is 35-45 °C, and more preferably, the dripping rate in step S3 is 15 mL h -1 , stirring speed is 500 rpm, stirring time is 3 h, and stirring temperature is 45 ℃.

[0015] Preferably, the aging temperature in step S4 is 35-45°C, and the aging time is 3-24 h. More preferably, the aging temperature in step S4 is 45°C, and the aging time is 12 h.

[0016] Preferably, the freeze-drying temperature in step S5 is -30 to -60 °C, and the freeze-drying time is 12 to 24 h. More preferably, the freeze-drying temperature in step S5 is -60 °C, and the freeze-drying time is 12 h.

[0017] The second aspect of the present invention provides a high surface sodium ion battery electrode, the battery electrode composition includes the surface passivated and air-stable Prussian blue analogue prepared as above.

[0018] The preparation method of the above-mentioned high-area sodium-ion battery electrode is as follows: a surface-passivated and air-stable Prussian blue analogue, a conductive agent and a binder are mixed at a ratio of 90:5:5 (wt%), the resulting mixture is transferred to a 2 mL swing tube, several 3 mm zirconium dioxide beads are added, and the mixture is fully shaken to obtain a uniform slurry, which is coated on aluminum foil and placed in a vacuum drying oven at 80 °C for 12 h to completely evaporate the solvent. After rolling on a double-roller machine, a sodium-ion battery high-area loading electrode with a certain compaction density is obtained, and then the pieces are cut and weighed to calculate the area loading mass and the active material loading amount.

[0019] Preparation method of high surface loading sodium ion battery electrode with compaction density of 1.4 g cm -3 -1.8 g cm -3 , preferably with a compacted density of 1.4 g cm -3 .

[0020] The preparation method of high surface loading sodium ion battery electrode is to weigh and calculate the surface loading of 14 mg cm -2 -22 mg cm -2 The optimal surface loading calculated by weighing is 14 mg cm -2 .

[0021] The conductive agent in the preparation method of high-surface sodium-ion battery electrodes can specifically adopt the currently common conductive agent raw materials used for battery electrodes, such as carbon black, acetylene black, Ketjen black, Super-P and carbon nanotubes, etc. The preferred conductive agent is Ketjen black.

[0022] The binder in the preparation method of high-surface sodium-ion battery electrodes can specifically adopt the currently common binder raw materials used for battery electrodes, such as polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, water-based glue, N-methyl-2-pyrrolidone, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer, fixed pump rubber, fluororubber and various copolymers. The preferred binder is a water-based glue.

[0023] The beneficial effects of the present invention are as follows: Preparation method: Prussian blue analogues are prepared by coprecipitation method. The raw materials are easily available, the metals contained are cheap, the process is simple, the production cost is low, and it has the potential for large-scale production. The Prussian blue analogues after surface passivation have good structural stability in the air and are not prone to phase change. At the same time, they can stabilize the interface, reduce side reactions, and improve cycle stability during the cycle process.

[0024] The prepared surface-passivated Prussian blue analogue exhibits good cycle capacity retention and rate performance in high-surface-loading positive electrode sheets, which is conducive to industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.

[0026] Figure 1 This is a thermogravimetric (TG) comparison chart of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention.

[0027] Figure 2 This is a scanning electron microscope (SEM) cross-sectional view of the high-surface electrode sheet prepared in Example 1-2 of the present invention. Figure 3 The electrode sheets of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention were -1 Comparison of cycling performance under different current densities.

[0028] Figure 4 It is a comparison chart of the rate performance of the electrode sheets of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention.

[0029] Figure 5 The electrode sheets of FHCF and PFHCF-2 prepared in Example 3 of the present invention were -1 Comparison of cycling performance under different current densities.

[0030] Figure 6 This is a Fourier transform infrared spectrum (FT-IR) comparison chart of the air stability of FHCF and PFHCF-2 prepared in Example 4 of the present invention.

[0031] Figure 7 This is a comparison chart of X-ray powder diffraction (XRD) of the air stabilities of FHCF and PFHCF-2 prepared in Example 4 of the present invention.

[0032] Figure 8 This is a Raman spectrum comparison chart of the air stability of FHCF and PFHCF-2 prepared in Example 4 of the present invention.

[0033] Fig. 9The air stability of the electrode sheets of FHCF and PFHCF-2 prepared in Example 4 of the present invention is 100 mAg -1 Comparison of cycling performance under different current densities. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any simple modification, equivalent changes and modifications made to the following examples based on the technical essence of the present invention still fall within the scope of the technical solution of the present invention.

[0035] Example 1, S1, sodium citrate (180 mmol) was dissolved in 100 mL of pure water, and then ferrous sulfate (40.5 mmol), zinc sulfate (4.5 mmol) and ascorbic acid (8.2 mmol) were dissolved in the above solution, and stirred on a constant temperature magnetic stirrer for 3 h, which was recorded as solution A.

[0036] S2, dissolve sodium ferrocyanide (45 mmol) in 100 mL of pure water and stir on a constant temperature magnetic stirrer for 3 h, which is recorded as solution B. The beaker containing 50 mL of pure water is recorded as solution C.

[0037] S3, solution A and solution B were respectively heated at 15 mL h -1 The solution was added dropwise at a rate of 1.50 μg / mL to a C solution at a constant temperature of 45 °C, stirred for 2 h, and aged for 12 h. The lower precipitate was then washed with water and ethanol several times, placed in a vacuum freeze dryer at -60 °C and freeze-dried for 12 h, and the surface-passivated Prussian blue analogue (denoted as PFHCF-2) was collected.

[0038] S4, preparation of electrode: PFHCF-2 material, Ketjen black (conductive agent) and water-based glue (binder) in step S3 were mixed at a ratio of 90:5:5 (wt%), and the resulting mixture was transferred to an oscillating tube. Six 3 mm zirconium dioxide beads were added and shaken thoroughly to obtain a uniform slurry. The slurry was evenly coated on aluminum foil using a coater (MSK-AFA-I), and placed in a vacuum drying oven at 100 °C for 12 h to allow the solvent to evaporate completely. The electrode was rolled by a roller machine to a compact density of 1.4 g cm -3 , cut into circular pole pieces with a diameter of 10 mm using a cutting machine (MSK-T10), and weigh the surface load to be 14 mg cm -2 .

[0039] S5, electrochemical performance test: All battery assemblies were completed in the inert atmosphere of the glove box (O2wt%≤0.01, H2Owt%≤0.01). The constant current charge and discharge test and long cycle test of CR2032 button cell were realized by NewareCT4000. The test voltage window was 2-4.0 V and the current density was 1C=100 mA g -1 For comparison, FHCF was prepared under the same conditions.

[0040] Example 2: The difference between this example and Example 1 is that the zinc sulfate in step ① is removed, and the content of ferrous sulfate is increased to 45 mmol. The other conditions are exactly the same as those in Example 1. The product (denoted as FHCF) is obtained and its electrochemical performance is tested.

[0041] Example 3: The difference between this example and examples 1 and 2 is that the weighing surface mass of the circular pole piece with a diameter of 10 mm is 22 mg cm -2 The other conditions are exactly the same as those in Example 1 and Example 2.

[0042] Example 4 In this example, the Prussian blue analogs FHCF and PFHCF-2 prepared in Example 1 and Example 3 were placed in the air for one month. The other conditions were exactly the same as steps S4 and S5 in Example 1.

[0043] Figure 1 This is a TG comparison chart of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention. It can be seen that PFHCF-2 contains less crystal water.

[0044] Figure 2 The SEM cross-sectional view of the high-surface electrode sheet prepared in Example 1-2 of the present invention shows that the -3 At a compacted density of 14 mg cm -2 and 22 mg cm -2 The mass-loaded pole pieces exhibit thicknesses of 78 μm and 136 μm, respectively.

[0045] Figure 3 The electrode sheets of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention were -1 From the comparison of cycle performance under current density, it can be seen that the capacity retention rate of PFHCF-2 is relatively high after 400 cycles.

[0046] Figure 4 The comparison diagram of the rate performance of the electrode sheets of FHCF and PFHCF-2 prepared in Examples 1-2 of the present invention shows that PFHCF-2 has a high rate performance at 750 mA g -1At a current density of 115 mAh g -1 capacity.

[0047] Figure 5 The electrode sheets of FHCF and PFHCF-2 prepared in Example 3 of the present invention were -1 From the comparison of cycle performance under current density, it can be seen that PFHCF-2 has high capacity and cycle retention rate.

[0048] Figure 6 The FTIR comparison chart of the air stability of FHCF and PFHCF-2 prepared in Example 4 of the present invention shows that after the sample has been placed for one month, the C≡N peak of FHCF has a red shift, indicating that the structure has changed, while PFHCF-2 has a stable structure.

[0049] Figure 7 The XRD comparison diagram of the air stability of FHCF and PFHCF-2 prepared in Example 4 of the present invention shows that after the sample has been placed for one month, the XRD peak of FHCF undergoes a phase change and a by-product Na4Fe(CN)6 is derived, indicating that the structure has changed, while PFHCF-2 exhibits a stable phase structure.

[0050] Figure 8 This is a Raman comparison of the air stability of FHCF and PFHCF-2 prepared in Example 4 of the present invention. It can be seen that after the sample has been placed for one month, the Raman peak of FHCF shifts to a high band, and the Fe 3+ Higher than Fe 2 + PFHCF-2 exhibits a relatively stable structure, and the product is mainly Fe 2+ Mostly.

[0051] Fig. 9 The air stability of the electrode sheets of FHCF and PFHCF-2 prepared in Example 4 of the present invention is 100 mA g -1 From the comparison of cycle performance under current density, it can be seen that after one month of storage, the capacity of FHCF decreased and the cycle stability was poor, while the capacity of PFHCF-2 remained almost unchanged and the cycle stability was good.

[0052] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, the equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A method for preparing a surface-passivated Prussian blue analogue, It is characterized in that The Prussian blue analogue is prepared by weighing a transition metal iron source, a surface passivation metal zinc source and a chelating agent according to a stoichiometric ratio, stirring and dissolving them in pure water to form a mixed solution; dropping the mixed solution into a sodium ferrocyanide solution, mixing evenly, and aging at the same temperature; taking a lower layer of precipitate, washing it with pure water and ethanol, and drying it to obtain a Prussian blue analogue.

2. A method for preparing a surface-passivated Prussian blue analogue according to claim 1, It is characterized in that The following steps are involved: S1, dissolving the chelating agent in pure water, then adding ferrous salt, zinc salt and ascorbic acid to the solution, wherein the concentration of the chelating agent is 0-2 mol L -1 , the concentration of zinc salt is 0-0.1 mol L -1 , the concentration of ascorbic acid is 0-0.2 mol L -1 , the concentration of ferrous salt is 0-0.5 mol L -1 ; S2, dissolving sodium ferrocyanide in pure water, wherein the concentration of sodium ferrocyanide is 0-0.5 mol L -1 ; S3, the solutions prepared in steps S1 and S2 were simultaneously heated at 10 mL h -1 -20 mL h -1 The mixture is dripped into a beaker containing 10-100 mL of water at a dripping rate of 400-500 rmp, the stirring time is 0.5-3 h, and the stirring temperature is 35-45 °C; S4, subjecting the mixed solution of step S3 to static aging, wherein the aging temperature is 35-45°C and the aging time is 3-24 h; S5, after the reaction is completed, the obtained product is centrifugally washed with deionized water and anhydrous ethanol for multiple times, and then freeze-dried in a vacuum, wherein the freeze-drying temperature is -30~-60°C and the freeze-drying time is 12-24 h, and finally a powdered Prussian blue analogue is obtained.

3. A method for preparing a surface-passivated Prussian blue analogue according to claim 2, It is characterized in that The chelating agent in step S1 is one or more of citric acid, sodium citrate, disodium ethylenediaminetetraacetic acid and sodium pyrophosphate.

4. A method for preparing a surface-passivated Prussian blue analogue according to claim 2, It is characterized in that The zinc salt in step S1 is one or more of zinc sulfate, zinc chloride, zinc phosphate and zinc nitrate.

5. A method for preparing a surface-passivated Prussian blue analogue according to claim 2, It is characterized in that The ferrous salt in step S1 is one or more of ferrous sulfate, ferrous chloride, ferrous nitrate and ferrous acetate.

6. A high surface loading sodium ion battery energy storage device, include: A high-surface-load positive electrode sheet, comprising a positive electrode current collector and a high-surface-load electrode material loaded on the current collector, a negative electrode sheet and a separator, characterized in that the high-surface-load electrode material comprises a surface-passivated and air-stable Prussian blue analogue obtained by the preparation method according to any one of claims 1-5.

7. A high surface area sodium ion battery energy storage device according to claim 6, It is characterized in that The surface loading of the high surface loading electrode is 14 mg cm -2 -22 mg cm -2 .

8. A high surface area sodium ion battery energy storage device according to claim 6, It is characterized in that The compacted density of the high surface loading electrode is 1.4 g cm -3 -1.8 g cm -3 .

9. A high surface area sodium ion battery energy storage device according to claim 6, It is characterized in that The thickness of the high-surface-loaded electrode is 70 μm-150 μm.

Citation Information

Patent Citations

  • Inert transition metal element doped iron-based Prussian blue sodium ion battery positive electrode material

    CN113104863A

  • Preparation method of Prussian blue analogue sodium ion battery positive electrode material

    CN116588953A

  • Preparation method of Prussian blue sodium ion battery positive electrode material with high capacity and long cycle performance

    CN117486233A

  • Preparation method and application of iron-based Prussian blue nano material

    CN117623336A

  • A portable press powder for latent fingerprints and method for preparing the same