Photo-thermal evaporation ion separation membrane, preparation method and application
Through the porous channel structure of the photothermal evaporation ion separation membrane, solar energy is used to drive lithium ions to separate from high magnesium lithium salts, solving the problems of complex lithium extraction process and large energy consumption, and achieving efficient and environmentally friendly lithium salt crystal collection and Separation.
Patent Information
- Application Number
- CN202411316378.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing lithium ions extracted from salt lake salt water is complex and has a large energy consumption, making it difficult to effectively deal with salt water with high magnesium-lithium ratio. The traditional nanofiltration process has the problems of high equipment and facilities investment and cumbersome operations.
A photothermal evaporation ion separation membrane is used, which includes a mass transfer layer and an ion separation layer. A porous channel is set on the mass transfer layer. The solar light is converted into a thermally driven ions through the ion separation layer to achieve selective separation of lithium and magnesium. The material layer is a hydrophilic or organic material and is suitable for water or organic solutions.
It realizes efficient, green and environmentally friendly lithium salt crystal collection, reduces operating costs, improves salt concentration capacity, has the separation factor up to more than 20, the crystallization rate of lithium chloride reaches 600mg/m2/h, and the device is simple and portable.
Smart Images

Figure CN119059596A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photothermal evaporation ion separation membrane, a preparation method and application thereof, and belongs to the field of ion separation. Background Art
[0002] Lithium (Li) has become one of the most valuable resources in the 21st century, and demand has increased dramatically due to its application in electric transportation batteries and sustainable energy storage. Procurement of lithium from various channels has become critical, among which lithium obtained from salt lake brine accounts for 70% of the lithium that can be mined on land, and it has become an important supply route to ensure the healthy development of the lithium battery market.
[0003] Lithium ion (Li + ) is abundant in salt lake brines, but compared with other coexisting cations, Li + The concentration of magnesium (Mg) is often one to three orders of magnitude higher than that of Li. In a typical process sequence for extracting Li (from brine), Li + In the final precipitation step, it is recovered as hydroxide or carbonate. Since Mg(OH)2 or MgCO3 also have low solubility, co-precipitation (LiOH or Li2CO3 precipitation) will occur during the precipitation process. Therefore, the key to achieving a high-purity final product is to be able to selectively and efficiently separate Li in the steps before the precipitation process. + and Mg 2 + .
[0004] Conventional lithium extraction processes based on solar evaporation / precipitation require the use of large amounts of chemicals and are not effective in processing lithium ions with high Mg content. 2+ / Li + Nanofiltration (NF) can selectively separate monovalent and divalent ions and has been widely used in Li ion separation due to its separation efficiency, modularity and process sustainability. + / Mg 2+ However, due to the high ionic strength, complex raw material composition, and easy scaling in salt lake water, it is very challenging to directly extract lithium using nanofiltration technology. Therefore, NF is usually integrated with other pretreatment and post-treatment unit processes to assemble a complete treatment process. The current typical integrated nanofiltration treatment process is: before the NF module treatment, the typical pretreatment process is to pre-enrich the Li in the original salt lake water through the sodium-potassium precipitation process module. The brine with a high magnesium-to-lithium ratio is diluted by a certain proportion and enters the NF process module to obtain a brine with a greatly reduced magnesium-to-lithium ratio, Li + Subsequently, a reverse osmosis membrane treatment process module is used as a post-treatment process to concentrate the Li in the permeate from the NF process module. +It is used in the final precipitation step and the clean water is recycled for dilution of high-concentration brine before treatment in the NF process module.
[0005] Such multi-unit collaborative treatment process is complex and cumbersome to operate. It involves high investment costs for equipment and facilities in the pressure-driven membrane treatment process section (nanofiltration membrane and reverse osmosis membrane treatment units) and huge energy consumption. Summary of the invention
[0006] In order to solve the problems existing in the existing separation of lithium and magnesium ions in the solution, the present invention provides a photothermal evaporation ion separation membrane, which can be used not only to separate lithium and magnesium ions in salt lake solutions to achieve lithium extraction, but also to separate other ions with different radii or different charges. The solution can be an aqueous solution or an organic solution. The separation membrane includes a mass transfer layer and an ion separation layer. The ion separation layer can separate ions in the solution by pore structure or charge properties, so that the required ions pass through the ion separation layer and the remaining ions are intercepted. The mass transfer layer is provided with nano-scale porous channels and has good compatibility with the solvent. If the solution is an aqueous solution, the mass transfer layer is a hydrophilic material. If the solution is an organic solution, the mass transfer layer is organic solvent-friendly. The porous channels in the mass transfer layer can generate capillary forces of more than 7 MPa, driving water to drive the ions to be separated to pass through the ion separation layer to the mass transfer layer. When in use, the lower surface of the ion separation layer (the side facing away from the mass transfer layer) is in contact with the solution, and the mass transfer layer is placed above the liquid surface of the solution. The absorbed light is converted into heat, and the water entering the mass transfer layer is heated to be converted into water vapor or the organic solvent is heated to be converted into gas to escape into the air, leaving the desired ions and depositing them in the porous channels of the mass transfer layer or on the upper surface of the mass transfer layer. After the ions accumulate to a certain amount, the ions in the mass transfer layer are removed by soaking, scraping or other methods.
[0007] The technical scheme adopted is: a photothermal evaporation separation membrane, including a mass transfer layer and an ion separation layer, the mass transfer layer is provided with dense porous channels, and can absorb sunlight and convert it into heat, the ion separation layer is a porous structure, which can pass the required ions and solvent molecules to separate the required ions from other ions, the average pore size of the ion separation layer is 0.4-0.5nm, the porous channels on the mass transfer layer are conducive to generating capillary forces on the one hand, thereby driving ions and solvents through the ion separation membrane to the mass transfer layer, and on the other hand, providing transmission channels for ions and solvents, the mass transfer layer is a hydrophilic material, and the porous channels thereon are preferably nanoscale channels, and more preferably channels with an average pore size of 8-12nm, the contact angle is 60-80°, preferably 72°, and further preferably, the average pore size is 10nm, which can not only provide megapascal osmotic pressure, but also facilitate the transmission of ions and water, and avoid ions deposited in the pores to block the pores, the porosity is 50-80%, preferably 60-70%, and the thickness of the mass transfer layer is preferably 240μm.
[0008] As a preferred solution, the mass transfer layer and the ion separation layer are an integrated structure. A solution that can be adopted is that at least one of the two is directly generated on the other membrane layer. This arrangement is conducive to the capillary force of the mass transfer layer to fully act on the ion separation layer, thereby achieving effective transmission of water and ions. As one implementation method, the ion separation membrane is generated on one side of the mass transfer layer, and then forms an integrated structure.
[0009] As a preferred embodiment, the photothermal evaporation ion separation membrane is used to separate ions in an aqueous solution, more preferably to separate ions of different valence states, and further preferably to separate monovalent ions and divalent ions.
[0010] As a preferred solution, the mass transfer layer is a mixed material of an organic polymer material and a light-absorbing material. The organic polymer material is conducive to forming a porous channel, and the pore size is adjustable, and has the advantages of hydrophilicity and adjustable hydrophilicity. After the light-absorbing material is compounded with the organic polymer material, the mass transfer layer can have a light-absorbing heat-conversion function. As a preferred solution, the organic polymer material is one of polyvinylidene fluoride, polyimide, polyether sulfone, polyester, polytetrafluoroethylene, cellulose acetate, polysulfone, and polyacrylonitrile. The light-absorbing material can be an organic or inorganic material, such as carbon nanotubes (CNTs), carbon black, carbon powder, graphene, and polyaniline. As a preferred combination, the organic polymer material is polyether sulfone and the light-absorbing material is polyaniline. The two have good compatibility and are evenly dispersed. In the phase inversion process, the two are conducive to forming a stable pore structure.
[0011] The present invention also provides a method for preparing the above-mentioned photothermal evaporation separation membrane: the method can be the following two methods: (1) first preparing a mass transfer layer, and then preparing an ion separation layer on the mass transfer layer; (2) first preparing an ion separation layer, and then preparing a mass transfer layer on the ion separation layer. Preferably, the mass transfer layer is prepared first, and then the ion separation layer is prepared by in-situ growth on one side of the mass transfer layer.
[0012] As a preferred solution, the preparation method of the mass transfer layer is as follows: select an organic polymer as the main body of the porous membrane, select a light absorbing material and the organic polymer to mix to form a porous membrane, and perform the following steps: (1) blend the organic polymer, the light absorbing material, and the additive in a solvent in a set amount to form a mixed solution; (2) mechanically stir the mixed solution, and let it stand after stirring to fully degas the solution, preferably, the standing time is 24 hours; (3) scrape the solution to form a film, preferably use a 250μm solution scraper to scrape a square liquid film with a side length of 10cm on a smooth glass plate in a casting manner; (4) then quickly immerse the liquid film in deionized water for non-solvent induced phase transformation, and continue to immerse for 24 hours to complete the phase transformation. Finally, the mass transfer layer is prepared.
[0013] As a preferred solution, the organic polymer is polyethersulfone, and its content in the mixed solution is 10-15wt%; the light absorbing material is polyaniline, and its content in the mixed solution ranges from 3-8wt%; the additives include non-solvent additives and liquid solvent additives, wherein the non-solvent additives are lithium chloride, polyethylene glycol (PEG) and polyvinylpyrrolidone (PVP). On the one hand, the three are conducive to improving the hydrophilicity of the mass transfer layer; on the other hand, the pore sizes formed by the three and polyethersulfone after the reaction are different, which is conducive to regulating the final pore size of the mass transfer layer so that it can generate megapascal pressure. In the present invention, preferably, lithium chloride, polyethylene glycol, polyvinyl pyrrolidone, the mass ratio of lithium chloride, polyethylene glycol, polyvinyl pyrrolidone is (1-5): (1-5): (1-5); more preferably, the dosage of the three in the polymer solution is 1-5wt%, lithium chloride and polyether sulfone can form a pore size of 10-50nm, PEG and polyether sulfone can form a pore size of 20-220nm, PVP and polyether sulfone can form a pore size of 50-220nm, under this mixing ratio, the final pore size formed is 8-12nm, and nanoscale pores are generated. Further preferably, the liquid solvent additives are glycerol and isopropanol, glycerol and isopropanol make the polymer solution close to its cloud point, and the hydroxyl groups in the molecules have a strong ability to form hydrogen bonds with water during the phase transformation film formation process, which promotes the exchange of solvent and water, causes instantaneous liquid-liquid phase separation, forms a porous membrane with higher porosity, and makes the pore size distribution of the polymer membrane narrower (the pore size distribution is more uniform). Preferably, the content of glycerol and isopropanol in the mixed solution is in the range of 3-5 wt %.
[0014] As a preferred solution, the solvent is N,N-dimethylformamide (DMF), and its content in the mixed solution ranges from 52 to 78 wt%. DMF has a relatively low boiling point and higher polymer solubility, and has more solid content ratio control options for PES polymers. In addition, DMF can replace water in the coagulation bath more quickly during the phase transformation of the polymer, and the porosity of the formed polymer film is higher.
[0015] Under the synergistic effect of polyethersulfone, polyaniline, lithium chloride, polyethylene glycol, polyvinyl pyrrolidone, glycerol, isopropanol and N,N-dimethylformamide, a black polymer membrane with an average pore size of 10 nm is finally formed.
[0016] As a preferred solution, the preparation method of the ion separation layer is as follows: S01 prepares an aqueous solution of piperazine and sodium dodecylbenzene sulfonate as the first solution; prepares a n-hexane solution of trimesoyl chloride as the second solution; S02 immerses one side of the mass transfer layer in the first solution, takes it out after immersion for a set time, and immerses it in the second solution for polymerization reaction, generates a polymer on the second surface, and obtains the ion separation layer. As a preferred method, the mass fraction of piperazine in the first solution is 0.1-5wt%, the mass fraction of sodium dodecylbenzene sulfonate is 0.1-3.6mmol / L, and the mass fraction of trimesoyl chloride in the second solution is 0.05-0.3wt%. Further preferably, the preparation method of the ion separation layer is as follows: (1) preparing an aqueous solution containing 0.1-5 wt% piperazine (PIP) and 0.1-3.6 mmol / L sodium dodecylbenzene sulfonate (SDBS), and magnetically stirring at 20-40° C. for 1-5 h to obtain a completely dissolved PIP aqueous solution; (2) preparing an n-hexane (n-Hexane) solution containing 0.05-0.3 wt% trimesoyl chloride (TMC), and magnetically stirring at 20-40° C. for 1-5 h to obtain a completely dissolved TMC n-hexane solution; (3) immersing one side of the mass transfer layer in the PIP aqueous solution for 0.5-10 min; (4) taking the mass transfer layer out of the PIP aqueous solution, removing excess water on the surface, and then immersing it in a n-hexane solution containing TMC for 10-360 s to perform an interfacial polymerization reaction. The specific reaction formula is as follows:
[0017] Wherein, ※ represents the entire piperazine or trimesoyl chloride monomer; polyamide is a polymer chain structure, which is a whole connected by two monomers alternately reacting together. The PIP monomer in the aqueous phase and the TMC monomer in the n-hexane solution undergo an irreversible rapid polycondensation reaction on the surface of the mass transfer layer, and finally form a dense membrane layer in situ on the surface of the mass transfer layer; (5) The mass transfer layer is taken out from the n-hexane solution of TMC and slowly rinsed with pure n-hexane for 1-5 minutes to remove unreacted chemicals; (6) The mass transfer layer with the polymer in situ is placed in an oven at 50-80°C for 1-3 hours, preferably at 50°C for 2 hours, to obtain an ion separation membrane layer formed integrally with the mass transfer layer, and the ion separation layer is a nanofiltration membrane layer; (7) The ion separation membrane is taken out from the oven and soaked in deionized water at room temperature for standby use. In order to improve the interception rate of the ion separation layer and the extraction efficiency of ions, in step (1), the mass fraction of PIP in the aqueous solution of PIP&SDBS is 2wt%, the concentration of SDBS is 1.2mmol / L, and the concentration of TMC in the n-hexane solution is 0.15wt%, and they are all stirred for 2h to obtain monomer solutions of aqueous phase and oil phase. The immersion time of the mass transfer layer in the aqueous phase solution and the oil phase solution is 1min and 30s, respectively. The ion separation layer prepared by this method is an integrated structure with the mass transfer layer. The ion separation layer has specific nanopores and surface charges, which can enable it to effectively intercept Mg in the salt solution. 2+ , while allowing most of Li + As water flows through the internal nanopores and migrates upward, Li + It is enriched inside and on the surface of the evaporation / mass transfer mixed layer. Preferably, the pore size of the ion separation layer is 0.4-0.8 nm, and the surface charge is -50 to -20 mV at pH = 6.5.
[0018] In order to make the ion separation membrane float on the liquid surface, the ion separation membrane is encapsulated between two O-rings. The gaskets not only play a supporting role, but also provide buoyancy, allowing the entire device to float on the liquid surface and ensure that the ion separation layer is in contact with the solution.
[0019] The beneficial effects of the present invention include:
[0020] (1) The ion separation membrane in the present invention uses interfacial photothermal evaporation to provide a driving force for the transmission of ions or solutes. It can use the capillary negative pressure of up to 100 MPa generated by the photothermal evaporation of liquid in the capillary channel to drive the underlying nanofiltration membrane to perform selective ion separation, thereby achieving green environmental protection while reducing operating costs. In addition, the photothermal effect is used to directly collect lithium salt crystals on the surface of the integrated photothermal evaporation-separation membrane. Compared with traditional membrane separation processing technology, the salt concentration capacity is greatly improved, and green, clean, cheap, and renewable lithium extraction from salt lakes is achieved.
[0021] (2) The ion separation membrane of the present invention can directly treat salt lake brine with high concentration and high magnesium-lithium ratio, and collect high-purity lithium salt crystals on the surface of the separation membrane. By adjusting the pore size and surface charge properties of the nanofiltration layer, the separation factor can reach more than 20, and the lithium chloride crystallization rate can reach 600 mg / m 2 / h or more. It can also achieve long-term stable operation, and lithium salt crystals can be recycled and collected, and it is economical and efficient.
[0022] (3) The mass transfer layer in the present invention has photothermal conversion, evaporation, and transmission functions, and can accurately control the appropriate photothermal conversion rate, pore size, and hydrophilic and hydrophobic properties according to the specific properties of the feed solution (such as the overall concentration of salt ions in the solution and the lithium-magnesium content ratio, etc.) to adapt to solutions of various properties;
[0023] (4) The ion separation layer in the present invention can be prepared in situ on either side of the mass transfer layer to form an integrated structure with the mass transfer layer, thereby transmitting capillary force without loss;
[0024] (5) The ion separation membrane of the present invention can be mass-produced and is portable (lightweight and thin), with a thickness of less than 0.5 mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Structural diagram of the photothermal evaporation ion separation membrane in the present invention;
[0026] Figure 2 A graph showing the water evaporation rate of the photothermal evaporation ion separation membrane in Example 1 in salt solutions of various concentrations;
[0027] Figure 3 The lithium-magnesium separation factor of the photothermal evaporation ion separation membrane in Example 1 in salt solutions of various concentrations;
[0028] Figure 4 The crystallization rate of lithium chloride of the photothermal evaporation ion separation membrane in salt solutions of various concentrations in Example 1;
[0029] Figure 5 A graph showing the water evaporation rate of the photothermal evaporation ion separation membrane in Example 1 in salt solutions with different lithium-magnesium ion mass ratios;
[0030] Figure 6 A bar graph of lithium-magnesium separation factors of the photothermal evaporation ion separation membrane in Example 1 in salt solutions with different lithium-magnesium ion mass ratios;
[0031] Figure 7 A graph showing the crystallization rate of lithium chloride of the photothermal evaporation ion separation membrane in Example 1 in salt solutions with different lithium-magnesium ion mass ratios;
[0032] In the figure, 1 is the mass transfer layer, and 2 is the ion separation layer. DETAILED DESCRIPTION
[0033] The present invention is further explained in detail below in conjunction with the accompanying drawings and specific embodiments, but it should be understood that the protection scope of the present invention is not limited to the specific embodiments.
[0034] Example 1
[0035] The photothermal evaporation ion separation membrane of the present invention is as follows Figure 1 , including a mass transfer layer 1 and an ion separation layer 2. The mass transfer layer 1 is provided with densely arranged pores, the pores are nanoscale, and can generate capillary force. The mass transfer layer 1 is made of hydrophilic material or the inner wall of the pores is made of hydrophilic material. Under the capillary force, water flows upward along the pores.
[0036] The ion separation layer can play the role of ion separation through pore size and / or charge, passing required ions and intercepting other ions. The ion separation layer in this embodiment passes lithium ions and intercepts divalent ions, such as magnesium ions.
[0037] When in use, the double-layer structure is fixedly connected around the membrane by rubber gaskets, so that the ion separation membrane floats on the surface of the solution, the mass transfer layer is the upper layer, and the ion separation layer is the lower layer. The ion separation layer is in contact with the solution and can be used to separate lithium ions and magnesium ions in the solution. When separating the two ions, lithium ions pass through the ion separation layer and deposit in the form of salt crystals on the top of the mass transfer layer, while most of the magnesium ions cannot pass through the ion separation layer. Finally, high-purity lithium ions are obtained by scraping or washing the top evaporation / mass transfer mixed layer, and the device can be reused for cyclic extraction of lithium salt crystals.
[0038] The device has a simple structure and excellent ion selective separation performance. With the help of the small-pore channels and photothermal conversion capabilities of the mass transfer layer, it can collect concentrated lithium salt crystals directly on the top of the mass transfer layer under solar energy drive.
[0039] The preparation method of the photothermal evaporation ion separation membrane comprises the following steps
[0040] S01 Preparation of mass transfer layer
[0041] A. A mixed polymer of polyethersulfone (PES) and polyaniline (PANI) is used as a main solidified film body, lithium chloride, polyethylene glycol (PEG) and polyvinyl pyrrolidone (PVP) are used as non-solvent additives, glycerol and isopropanol are used as liquid solvent additives, and N,N-dimethylformamide (DMF) is used as a solvent. The above film body materials, non-solvent additives and liquid solvent additives are mixed in a solvent to form a mixed solution; the mass fractions of the components in the mixed solution are: 12wt% PES, 8wt% PANI, 2wt% lithium chloride, 4wt% PEG, 2wt% PVP, 2wt% glycerol, 5wt% isopropanol, and 65wt% DMF;
[0042] The mixed solution B was mechanically stirred at 50°C for 15 h, and then allowed to stand for 24 h to complete the degassing of the solution;
[0043] C. Use a 250 μm solution doctor blade to apply a square liquid film with a side length of 10 cm on a smooth glass plate in a casting manner;
[0044] D The liquid membrane was then quickly immersed in deionized water for non-solvent-induced phase transformation, and the immersion was continued for 24 hours to complete the phase transformation; a black mass transfer layer was obtained, the average pore size of the pores was 10 nm, and the porosity measured by the weight method was 62%.
[0045] S02 Preparation of ion separation layer
[0046] (1) preparing an aqueous solution containing 2 wt % piperazine (PIP) and 0.15 mmol / L sodium dodecylbenzene sulfonate (SDBS), and magnetically stirring at 35° C. for 2 h to obtain a completely dissolved PIP aqueous solution;
[0047] (2) preparing a n-hexane solution containing 0.15 wt% trimesoyl chloride (TMC), stirring under magnetic force at 35° C. for 2 h, and obtaining a completely dissolved TMC n-hexane solution;
[0048] (3) With the upper surface of the mass transfer layer as the first surface and the lower surface as the second surface, the second surface of the mass transfer layer is immersed in the PIP aqueous solution for 1 min, and then taken out to remove excess water on the surface;
[0049] (4) Immerse the second surface in a hexane solution containing TMC for 30 seconds to perform an interfacial polymerization reaction. The polymerization reaction formula is:
[0050]
[0051] During the reaction, the PIP monomer in the aqueous phase and the TMC monomer in the n-hexane solution undergo an irreversible rapid condensation reaction on the second surface of the mass transfer layer, and finally a dense ion separation layer is formed in situ on the surface of the mass transfer layer. The average pore size of the ion separation layer characterized by the neutral molecule interception method is 0.42nm.
[0052] (5) taking out the mass transfer layer after the surface polymerization is completed from the n-hexane solution containing TMC, and slowly rinsing it with pure n-hexane for 1 min to remove the unreacted chemicals, thereby obtaining a photothermal evaporation ion separation membrane;
[0053] (6) placing the photothermal evaporation ion separation membrane in a 50° C. oven for 2 h to dry;
[0054] (7) The ion separation membrane is taken out from the oven and immersed in deionized water at room temperature. When it is used, it is taken out, packaged, and then floated on the solution.
[0055] Test Results
[0056] Prepare the following solution:
[0057] Solution 1: The salt solution is a mixed salt solution of magnesium chloride and lithium chloride with a total concentration of 80 g / L, wherein the mass ratio of lithium ions to magnesium ions is 1:1.
[0058] Solution two:
[0059] The salt solution is a mixed salt solution of magnesium chloride and lithium chloride with a total concentration of 10 g / L, wherein the mass ratio of lithium ions to magnesium ions is 1:1.
[0060] Solution three:
[0061] The salt solution is a mixed salt solution of magnesium chloride and lithium chloride with a total concentration of 20 g / L, wherein the mass ratio of lithium ions to magnesium ions is 1:1.
[0062] Solution four:
[0063] The salt solution is a mixed salt solution of magnesium chloride and lithium chloride with a total concentration of 30 g / L, wherein the mass ratio of lithium ions to magnesium ions is 1:1.
[0064] Solution 5:
[0065] The salt solution is a mixed salt solution of magnesium chloride and lithium chloride with a total concentration of 40 g / L, wherein the mass ratio of lithium ions to magnesium ions is 1:1.
[0066] Solution 6:
[0067] The mass ratio of lithium to magnesium ions is 10:1, and the total concentration of the mixed brine solution of fixed magnesium chloride and lithium chloride is 10 g / L.
[0068] Solution seven:
[0069] The mass ratio of lithium to magnesium ions was fixed at 20:1, and the total concentration of the mixed brine solution of magnesium chloride and lithium chloride was fixed at 10 g / L.
[0070] Solution eight:
[0071] The mass ratio of lithium to magnesium ions was fixed at 40:1, and the total concentration of the mixed brine solution of magnesium chloride and lithium chloride was fixed at 10 g / L.
[0072] Solution Nine:
[0073] The mass ratio of lithium to magnesium ions was fixed at 80:1, and the total concentration of the mixed brine solution of magnesium chloride and lithium chloride was fixed at 10 g / L.
[0074] Solution ten:
[0075] The mass ratio of lithium to magnesium ions was fixed at 160:1, and the total concentration of the mixed brine solution of magnesium chloride and lithium chloride was fixed at 10 g / L.
[0076] The above solutions were poured into square boxes of 20cm*20cm*10cm respectively, and the square boxes corresponding to solution 1 to solution 10 were square box 1 to square box 10 respectively. The photothermal evaporation ion separation membrane obtained in Example 1 was placed on the square boxes corresponding to each solution. The photothermal evaporation ion separation membrane floated on the solution, and the ion separation layer was in contact with the solution. The top mass transfer layer generated a capillary force of 100 MPa due to the presence of nanoscale pores, and the pressure was transmitted to the ion separation layer to start driving the membrane filtration, thereby selectively intercepting Mg. 2+ and through Li + This part of lithium salt finally crystallizes and precipitates at the top of the mass transfer layer. It can be directly collected by brushing (or dissolved and collected by washing). The whole test time is 24 hours, and the precipitation of lithium salt crystals can be seen at the top of the mass transfer layer under the irradiation of 3 suns.
[0077] The water evaporation rate, separation factor and lithium chloride crystallization rate in the corresponding square boxes of test solutions 1 to 5 are as follows: Figure 2 , Figure 3 and Figure 4 .Depend on Figure 2 and Figure 3 As shown in the figure, with the increase of the mixed salt solution of magnesium chloride and lithium chloride, the water evaporation rate and separation factor remain basically unchanged, indicating that the photothermal evaporation ion separation membrane can be applied to salt solutions of various concentrations, and the separation efficiency is not affected by the concentration of the salt solution. Figure 4 As shown, with the increase of the mixed salt solution of magnesium chloride and lithium chloride, the crystallization rate of lithium chloride increases, indicating that high concentration salt solution is beneficial to improving the crystallization rate of lithium chloride.
[0078] The water evaporation rate, separation factor and lithium chloride crystallization rate in the test solution six to ten square boxes are as follows Figure 5 , Figure 6 and Figure 7 .Depend on Figure 5 and Figure 6 As shown, when the total concentration of the mixed brine solution of magnesium chloride and lithium chloride is fixed at 10 g / L, as the mass ratio of lithium to magnesium ions increases, the water evaporation rate remains basically unchanged, while the separation factor gradually increases, indicating that the photothermal evaporation ion separation membrane can be used for salt solutions with various magnesium-to-lithium mass ratios, and the separation efficiency is not affected by the magnesium-to-lithium mass ratio in the salt solution. Figure 7 As shown, with the increase of the mass ratio of magnesium to lithium in the mixed salt solution of magnesium chloride and lithium chloride, the crystallization rate of lithium chloride gradually decreases. This is because the mass fraction of lithium ions in the mixed salt solution decreases significantly, but the crystallization rate of lithium chloride is still high.
[0079] The separation factor is obtained as follows: separation factor = mass ratio of lithium and magnesium ions after separation / mass ratio of lithium and magnesium ions before separation. If the mass ratio of lithium and magnesium ions in the mixed solution to be separated is 1:1, in this embodiment, assuming that the mass ratio of lithium and magnesium ions entering the salt reservoir is 20:1 (the mass of magnesium and lithium ions in the salt reservoir can be measured by an inductively coupled plasma spectrometer), then the separation ratio is (20:1) / (1:1)=20.
[0080] The lithium chloride crystallization rate is the mass of lithium chloride powder collected on the top of the mass transfer layer by the interface evaporation driven by solar energy per unit area of the separation membrane per unit time. In the present invention, the salt crystal powder collected on the top of the mass transfer layer is dissolved in a certain volume of aqueous solution, and the mass concentration of lithium ions in the solution can be known by testing the aqueous solution with an inductively coupled plasma spectrometer. For example, the test value is 1 mg / L. Assuming that the volume of the aqueous solution is 0.1 L, it can be known that the mass of lithium in the salt crystals collected on the top of the evaporation / mass transfer mixed layer is 0.1 mg. The mass is converted by the molar mass ratio of lithium chloride and then divided by the working area and working time of the separation membrane to finally obtain the lithium chloride crystallization rate.
[0081] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A photothermal evaporation separation membrane, characterized in that: It includes a mass transfer layer and an ion separation layer; The mass transfer layer is provided with porous channels, and the mass transfer layer absorbs light and converts it into heat; The ion separation layer is arranged on one side of the mass transfer layer, and the ion separation layer selectively transmits the ions to be separated; When in use, the photothermal evaporation separation membrane is placed on the liquid surface, the ion separation layer contacts the solution, the porous channel generates capillary force, the solvent and the ions to be separated in the solution pass through the ion separation layer to the mass transfer layer, the solvent absorbs heat in the mass transfer layer and converts into gas to escape, and the ions to be separated are deposited in the pores of the mass transfer layer or on the surface of the mass transfer layer.
2. The photothermal evaporation separation membrane according to claim 1, characterized in that: The mass transfer layer and the ion separation layer are an integrated structure, the ion separation layer is grown on one side of the mass transfer layer, or the mass transfer layer is grown on one side of the ion separation layer.
3. The photothermal evaporation separation membrane according to claim 1, characterized in that: The solution is an aqueous solution of organic or inorganic salts, the pore size of the porous channels on the mass transfer layer is 8-12 nm, and the contact angle of the mass transfer layer is 25-80°.
4. The photothermal evaporation separation membrane according to claim 1, characterized in that: The material of the mass transfer layer is a mixed material formed by an organic polymer material and a light-absorbing material. The organic polymer material is a combination of one or more of polyvinylidene fluoride, polyimide, polyether sulfone, polyester, polytetrafluoroethylene, cellulose acetate, polysulfone, and polyacrylonitrile. The light-absorbing material is an organic and / or inorganic light-absorbing material.
5. A method for preparing a photothermal evaporation separation membrane according to claim 1, characterized in that: The following steps are involved: preparing a mass transfer layer, and growing an ion separation layer on one side of the mass transfer layer; Alternatively, an ion separation layer is prepared, and a mass transfer layer is grown on one side of the ion separation layer.
6. The method for preparing a photothermal evaporation separation membrane according to claim 5, characterized in that: A mass transfer layer is prepared, and an ion separation layer is prepared by in-situ growth on one side of the mass transfer layer, comprising the following steps: A mass transfer layer is prepared, wherein the mass transfer layer is a gel, and the preparation method of the mass transfer layer is as follows: S01: blending an organic polymer material for forming a gel and a light absorbing material in a solvent to form a mixed solution; S02: mechanically stirring the mixed solution and allowing it to stand for degassing; S03 After degassing is completed, the solution is formed into a liquid film, and then the liquid film is immersed in water to induce phase inversion to obtain the gel-state mass transfer layer; Taking the mass transfer layer as a substrate, an ion separation layer is prepared on one side of the mass transfer layer. The preparation method of the ion separation layer includes: S01: preparing an aqueous solution of piperazine and sodium dodecylbenzene sulfonate as a first solution; preparing a n-hexane solution of trimesoyl chloride as a second solution; S02: immersing one side of the mass transfer layer in a first solution, taking it out after immersion for a set time and immersing it in a second solution for polymerization reaction, generating a polymer on the second surface, and obtaining an ion separation layer.
7. The method for preparing a photothermal evaporation ion separation membrane according to claim 6, characterized in that: The mass fraction of piperazine in the first solution is 0.1-5wt%, the mass fraction of sodium dodecylbenzenesulfonate is 0.1-3.6mmol / L, and the mass fraction of trimesoyl chloride in the second solution is 0.05-0.3wt%.
8. The preparation method according to claim 6, characterized in that: The organic polymer is polyethersulfone, the light absorbing material is polyaniline, and the mass content of the polyethersulfone in the mixed solution is (10-15)%, and the mass content of the polyaniline is (3-8)%.
9. The method for preparing a photothermal evaporation ion separation membrane according to claim 6, characterized in that: Step S01 is: blending an organic polymer material for forming a gel, a light absorbing material, and an additive in a solvent to form a mixed solution, wherein the additive comprises one of the following: ——The additive is a non-solvent additive; ——The additive is a liquid solvent additive; ——The additives include non-solvent additives and liquid solvent additives. The non-solvent additive is lithium chloride, polyethylene glycol, and polyvinyl pyrrolidone, and the mass ratio of lithium chloride, polyethylene glycol, and polyvinyl pyrrolidone is (1-5): (1-5): (1-5); The liquid solvent additives are glycerol and isopropanol, and the mass ratio of glycerol to isopropanol is (3-5): (3-5).
10. The preparation method according to claim 6, characterized in that: The porosity of the mass transfer layer is 50-80%; the thickness of the ion separation layer is 100-200nm.
11. A use of a photothermal evaporation ion separation membrane, characterized in that: Lithium is extracted using the photothermal evaporation ion separation membrane according to claim 1, wherein the ion separation layer allows lithium ions to pass through and magnesium ions to be retained, and the photothermal evaporation ion separation membrane is placed in a lithium-containing solution, and the mass transfer layer is hydrophilic. Under the capillary force provided by the mass transfer layer, water and lithium ions pass through the ion separation layer to the mass transfer layer, water evaporates in the mass transfer layer, and lithium ions are deposited in the pores or on the surface of the mass transfer layer.
Citation Information
Patent Citations
High-water-flux forward-osmosis composite membrane and preparation method thereof
CN103977718A
Polysulfone-based photothermal conversion composite membrane for solar water evaporation and preparation method thereof
CN112128996A
Preparation method of high-selectivity lithium-magnesium separation membrane
CN113893713A
Ion separation device, method and application
CN115353247A
Composite nanofiltration membrane with low molecular weight cut-off and narrow pore size distribution and preparation method thereof
CN116036896A