Chloride ion erosion resistant recycled coarse and fine aggregate concrete and preparation method thereof
By adopting specific component proportions and process flow in recycled aggregate concrete, combining wollastonite and slag powder, the problem of insufficient chloride ion permeability of recycled aggregate concrete is solved, and the chloride ion corrosion resistance and mechanics of concrete are significantly improved Performance achieves the dual benefits of resource utilization and environmental protection.
Patent Information
- Application Number
- CN202411172709.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing recycled aggregate concrete has poor chloride ion permeability and cannot effectively alleviate the problem of insufficient mechanical properties and durability in the resource utilization of construction waste.
Using specific component ratios and process flow, including premixing and stirring of recycled coarse aggregates, recycled fine aggregates, natural gravel and natural sand and soaking in water, combining wollastonite and slag powder, and precisely controlling the effective water-glue ratio and microporous structure to improve the chloride ion corrosion resistance and mechanical properties of concrete.
It significantly improves the anti-chlorine ion erosion, mechanical properties and durability of concrete, reduces its dependence on natural ore resources, has significant environmental protection and economic value, and ensures the long-term durability and construction performance of concrete.
Smart Images

Figure BDA0005009778190000011 
Figure BDA0005009778190000031 
Figure BDA0005009778190000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to a recycled coarse and fine aggregate concrete resistant to chloride ion corrosion and a preparation method thereof. Background Art
[0002] With the acceleration of global urbanization, the demolition and construction of a large number of buildings has led to a rapid increase in construction waste. If construction waste is not effectively treated, it will not only occupy land resources, but also cause serious damage to the ecological environment. Therefore, how to recycle construction waste and apply it to concrete production has become an important topic in the field of building materials research.
[0003] The use of recycled aggregates can effectively reduce the demand for natural sand and gravel mining and alleviate the problem of resource shortage. However, due to the low quality of recycled aggregates, the concrete prepared with them has obvious deficiencies in mechanical properties and durability, especially its resistance to chloride ion penetration needs to be further improved. Summary of the invention
[0004] The problem in the prior art is that the recycled aggregate concrete prepared by conventional methods has poor resistance to chloride ion penetration. In view of the above problem, the present invention provides a recycled coarse and fine aggregate concrete resistant to chloride ion corrosion, which comprises the following components in parts by weight:
[0005]
[0006] Preferably, it is characterized in that the volume ratio of the recycled coarse aggregate to natural crushed stone is 7:3, and the volume ratio of the recycled fine aggregate to natural sand is 7:3.
[0007] Preferably, the weight ratio of the cement to wollastonite and slag powder is 36-38:70-90:70-90, and the weight ratio of the wollastonite to slag powder is 1:1.
[0008] Preferably, the ratio of the weight of water to the total weight of cement, wollastonite and slag powder is 15-17:50-56.
[0009] Preferably, the natural gravel is limestone gravel specified in GB / T14685-2022, with an average particle size of 4.75-21.50 mm; the natural sand is river sand specified in GB / T14684-2022, with an average particle size of 0.15-4.75 mm.
[0010] Preferably, the recycled coarse aggregate is recycled coarse aggregate of Class III and above as specified in GB / T25177-2010; and the recycled fine aggregate is recycled fine aggregate of Class III and above as specified in GB / T25176-2010.
[0011] Preferably, the cement is P.042.5 Portland cement.
[0012] Preferably, the SiO in the wollastonite 2 Content ≥95%, specific surface area ≥20m 2 / g, loss on ignition ≤1.51%.
[0013] Preferably, the slag powder is S105 grade slag powder with a loss on ignition ≤1.0%.
[0014] Preferably, the water reducing agent is a polycarboxylic acid high performance water reducing agent with a water reducing efficiency of 40%.
[0015] Preferably, the preparation method of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion comprises the following steps:
[0016] (1) Adding the formulated amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 75-100 rpm for 40 seconds, then adding 50% of the formulated amount of water, and stirring at 75-100 rpm for another 40 seconds to obtain an aggregate mixture;
[0017] (2) The aggregate mixture is placed in a sealed container and allowed to stand for 24 hours to obtain a prepreg aggregate mixture;
[0018] (3) adding all the prepreg aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 75-100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 75-100 rpm for another 40 seconds to obtain a concrete mixture;
[0019] (4) Place the concrete mixture into the mold and vibrate it on a vibration table for 20 seconds;
[0020] (5) placing the concrete mixture obtained in step (4) in a cool place indoors and leaving it to stand for 24 hours;
[0021] (6) After demolding, the concrete mixture of step (5) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 20±2° C. and the curing relative humidity is 93±3%.
[0022] The present invention has the following beneficial effects:
[0023] (1) The present invention first premixes recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand to form an aggregate mixture, then soaks it in water so that the aggregate mixture fully absorbs water to obtain a prepreg aggregate mixture, and then mixes the prepreg aggregate mixture with other raw materials. This process enables the obtained concrete to have better resistance to chloride ion corrosion. At the same time, by accurately controlling the effective water-binder ratio, the strength and durability of the obtained concrete during the construction process are ensured;
[0024] (2) The present invention uses a scientific combination of recycled aggregate and natural aggregate. This combination not only greatly reduces the dependence on natural mineral resources, has significant environmental protection benefits, but also has high economic value and supports multi-generation recycling. The addition of natural aggregate effectively optimizes the gradation of recycled aggregate, significantly improves the problem of high water absorption of recycled aggregate, and thus improves the working performance, mechanical properties and durability of concrete;
[0025] (3) The present invention pre-mixes and stirs recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand and then soaks them in water, which can fully peel off the weaker parts of the recycled aggregate. At the same time, the removed old mortar can fill the pores in the concrete, thereby further improving the density and chloride ion corrosion resistance of the obtained concrete;
[0026] (4) The rounded shape of natural aggregates enhances the interlocking effect between aggregates. The interlocking effect of aggregates has a significant impact on the performance of concrete by enhancing the compressive, tensile and flexural strength of concrete, improving durability and volume stability. The interlocking effect makes the aggregates tightly bonded, reduces porosity, improves impermeability and resistance to chloride ion erosion, and reduces the risk of shrinkage cracks. However, an excessively strong interlocking effect may affect the workability of concrete. Therefore, when designing the concrete mix ratio, it is necessary to strike a balance between mechanical properties and workability.
[0027] (5) The concrete of the present invention achieves multiple reinforcement mechanisms by adding silica fume and slag powder. These fine admixtures effectively fill the pores in the cement matrix through nucleation, filling and bridging, optimize the microscopic pore structure of the concrete, and effectively connect and repair microcracks to inhibit further expansion of the cracks. In addition, admixtures of different particle sizes form a good particle gradation, showing a "complementary advantage effect" and producing a super-composite superposition effect, thereby further improving the overall performance of the concrete, especially in terms of durability and resistance to chloride ion corrosion;
[0028] (6) The ion-corrosion-resistant recycled coarse and fine aggregate concrete obtained by the present invention has a slump of ≥180 mm, a compressive strength of 50 MPa or more, and a non-steady-state chloride ion rapid migration coefficient of ≤2.8×10-12 m 2 / s, and its resistance to chloride ion corrosion is very excellent, which can effectively prevent chloride ions from corroding the internal structure of concrete and ensure the long-term durability of concrete. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0030] The waste concrete recycled coarse aggregate used in the following embodiments of the present invention is Class III recycled coarse aggregate specified in GB / T25177-2010;
[0031] The waste concrete recycled fine aggregate used in the following embodiments of the present invention is Class III recycled fine aggregate specified in GB / T25176-2010;
[0032] The cement used in the following examples of the present invention is P.0 42.5 Portland cement.;
[0033] The wollastonite used in the following embodiments of the present invention has a brand name: Borun, model number WGF-6018;
[0034] The slag powder used in the present invention is S105 grade slag powder, and the loss on ignition is ≤1.0%. Brand: Longze, model LZ-001;
[0035] Unless otherwise specified, the raw materials used in the present invention are commonly available in the market.
[0036] Example 1
[0037] A recycled coarse and fine aggregate concrete resistant to chloride ion corrosion, which comprises the following components in parts by weight:
[0038]
[0039]
[0040] In the above formula, the volume ratio of 690 parts of recycled coarse aggregate to 330 parts of natural crushed stone is 7:3, and the volume ratio of 400 parts of recycled coarse aggregate to 190 parts of natural sand is 7:3.
[0041] The natural crushed stone is limestone crushed stone specified in GB / T14685-2022, with an average particle size of 4.75 mm;
[0042] The natural sand is river sand specified in GB / T14684-2022, with an average particle size of 0.15 mm;
[0043] The preparation method of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion is as follows:
[0044] (1) adding the formula amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 75 rpm for 40 seconds, then adding 50% of the formula amount of water, and stirring at 75 rpm for another 40 seconds to obtain an aggregate mixture;
[0045] (2) The aggregate mixture is placed in a sealed container and allowed to stand for 24 hours to obtain a prepreg aggregate mixture;
[0046] (3) adding all the aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 100 rpm for another 40 seconds to obtain a concrete mixture;
[0047] (4) Place the concrete mixture into the mold and vibrate it on a vibration table for 20 seconds;
[0048] (5) placing the concrete mixture obtained in step (4) in a cool place indoors and leaving it to stand for 24 hours;
[0049] (6) After demoulding, the concrete mixture of step (5) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 20° C. and the curing relative humidity is 93%.
[0050] Example 2
[0051] A recycled coarse and fine aggregate concrete resistant to chloride ion corrosion, which comprises the following components in parts by weight:
[0052]
[0053] In the above formula, the volume ratio of 660 parts of recycled coarse aggregate to 300 parts of natural crushed stone is 7:3, and the volume ratio of 370 parts of recycled coarse aggregate to 160 parts of natural sand is 7:3.
[0054] The natural crushed stone is limestone crushed stone specified in GB / T14685-2022, with an average particle size of 10 mm;
[0055] The natural sand is river sand specified in GB / T14684-2022, with an average particle size of 2 mm;
[0056] The preparation method of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion is as follows:
[0057] (1) adding the formula amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 100 rpm for 40 seconds, then adding 50% of the formula amount of water, and stirring at 100 rpm for another 40 seconds to obtain an aggregate mixture;
[0058] (2) The aggregate mixture is placed in a sealed container and allowed to stand for 24 hours to obtain a prepreg aggregate mixture;
[0059] (3) adding all the aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 75 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 75 rpm for another 40 seconds to obtain a concrete mixture;
[0060] (4) Place the concrete mixture into the mold and vibrate it on a vibration table for 20 seconds;
[0061] (5) placing the concrete mixture obtained in step (4) in a cool place indoors and leaving it to stand for 24 hours;
[0062] (6) After demoulding, the concrete mixture of step (5) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 22° C. and the curing relative humidity is 95%.
[0063] Example 3
[0064] A recycled coarse and fine aggregate concrete resistant to chloride ion corrosion, which comprises the following components in parts by weight:
[0065]
[0066] In the above formula, the volume ratio of 720 parts of recycled coarse aggregate to 360 parts of natural crushed stone is 7:3, and the volume ratio of 430 parts of recycled coarse aggregate to 220 parts of natural sand is 7:3.
[0067] The natural crushed stone is limestone crushed stone specified in GB / T14685-2022, with an average particle size of 21.5 mm;
[0068] The natural sand is river sand specified in GB / T14684-2022, with an average particle size of 4.75 mm;
[0069] The preparation method of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion is as follows:
[0070] (1) Adding the formula amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 90 rpm for 40 seconds, then adding 50% of the formula amount of water, and stirring at 80 rpm for 40 seconds to obtain an aggregate mixture;
[0071] (2) The aggregate mixture is placed in a sealed container and allowed to stand for 24 hours to obtain a prepreg aggregate mixture;
[0072] (3) adding all the aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 100 rpm for another 40 seconds to obtain a concrete mixture;
[0073] (4) Place the concrete mixture into the mold and vibrate it on a vibration table for 20 seconds;
[0074] (5) placing the concrete mixture obtained in step (4) in a cool place indoors and leaving it to stand for 24 hours;
[0075] (6) After demoulding, the concrete mixture of step (5) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 21° C. and the curing relative humidity is 90%.
[0076] Comparative Example 1 is the same as Example 1, except that the preparation method of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion in Comparative Example 1 is as follows:
[0077] (1) Putting the formulated amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone, natural sand, and 50% of the formulated amount of water into a sealed container and leaving it to stand for 24 hours to obtain a prepreg aggregate mixture;
[0078] (2) adding all the aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 100 rpm for another 40 seconds to obtain a concrete mixture;
[0079] (3) Load the concrete mixture into the mold and place it on a vibration table for 20 seconds;
[0080] (4) placing the concrete mixture obtained in step (3) in a cool place indoors and leaving it to stand for 24 hours;
[0081] (5) After demoulding, the concrete mixture of step (4) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 20° C. and the curing relative humidity is 93%.
[0082] Comparative Example 2 is the same as Example 1, except that the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion in Comparative Example 2 is prepared by the following method:
[0083] (1) adding the formula amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 75 rpm for 40 seconds, then adding 50% of the formula amount of water, and stirring at 75 rpm for another 40 seconds to obtain an aggregate mixture;
[0084] (2) adding the aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 100 rpm for another 40 seconds to obtain a concrete mixture;
[0085] (3) Load the concrete mixture into the mold and place it on a vibration table for 20 seconds;
[0086] (4) placing the concrete mixture obtained in step (3) in a cool place indoors and leaving it to stand for 24 hours;
[0087] (5) After demoulding, the concrete mixture of step (4) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 20° C. and the curing relative humidity is 93%.
[0088] Comparative Example 3 is the same as Example 1, except that the amount of recycled coarse aggregate added in Comparative Example 3 is 720 parts, and the volume ratio of the recycled coarse aggregate to natural crushed stone is 8:2.
[0089] Comparative Example 4 is the same as Example 1, except that the amount of recycled coarse aggregate added in Comparative Example 4 is 660 parts, and the volume ratio of the recycled coarse aggregate to natural crushed stone is 6:4.
[0090] Comparative Example 5 is the same as Example 1, except that the amount of recycled fine aggregate added in Comparative Example 5 is 430 parts, and the volume ratio of the recycled fine aggregate to natural sand is 8:2.
[0091] Comparative Example 6 is the same as Example 1, except that the amount of recycled fine aggregate added in Comparative Example 6 is 370 parts, and the volume ratio of the recycled fine aggregate to natural sand is 6:4.
[0092] Comparative Example 7 is the same as Example 1, except that no slag powder is added in Comparative Example 7, and the weight portion of wollastonite added is 160 parts.
[0093] Comparative Example 8 is the same as Example 1, except that wollastonite is not added in Comparative Example 8, and the weight portion of slag powder added is 160 parts.
[0094] Comparative Example 9 is the same as Example 1, except that the weight parts of water added in Comparative Example 9 is 100 parts.
[0095] Comparative Example 10 is the same as Example 1, except that the weight portion of cement added in Comparative Example 10 is 300 parts.
[0096] Comparative Example 11 is the same as Example 1, except that in Comparative Example 11, the weight proportion of wollastonite added is 50 parts, and the weight proportion of slag powder added is 90 parts.
[0097] Performance Testing
[0098] The performance test results of the recycled coarse and fine aggregate concrete resistant to chloride ion corrosion obtained in Examples 1-3 of the present invention and Comparative Examples 1-11 are shown in Table 1.
[0099] The present invention tests the physical properties of coarse aggregate according to GB / T14685-2022 "Crushed Stone and Pebbles for Construction".
[0100] The present invention determines the classification of recycled coarse aggregate according to GB / T25177-2010 "Recycled coarse aggregate for concrete".
[0101] The present invention tests the physical properties of fine aggregate according to GB / T14684-2022 "Construction Sand".
[0102] The present invention determines the classification of recycled fine aggregate according to GB / T25176-2010 "Recycled Fine Aggregate for Concrete and Mortar".
[0103] The present invention tests the slump of recycled fine aggregate concrete according to GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures".
[0104] The present invention tests the 28d compressive strength, splitting tensile strength and flexural strength of recycled fine aggregate concrete according to GB / T50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete".
[0105] The present invention tests the chloride ion penetration resistance of recycled fine aggregate concrete according to GB / T 50082 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete".
[0106] Table 1
[0107]
[0108] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A recycled coarse and fine aggregate concrete resistant to chloride ion corrosion, characterized in that: In parts by weight, it includes the following components: 660-720 parts of recycled coarse aggregate; 370-430 parts of recycled fine aggregate; 300-360 parts of natural crushed stone; 160-220 parts of natural sand; 360-380 parts of cement; Wollastonite 70-90 parts; 70-90 parts of slag powder; 2.72 parts of water reducing agent; 150-170 parts of water.
2. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The volume ratio of the recycled coarse aggregate to natural crushed stone is 7:3, and the volume ratio of the recycled fine aggregate to natural sand is 7:
3.
3. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The weight ratio of the cement to wollastonite and slag powder is 36-38:70-90:70-90, and the weight ratio of the wollastonite to slag powder is 1:
1.
4. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The ratio of the weight of the water to the total weight of the cement, wollastonite and slag powder is 15-17:50-56.
5. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The natural gravel is limestone gravel specified in GB / T14685-2022, with an average particle size of 4.75-21.50 mm; the natural sand is river sand specified in GB / T14684-2022, with an average particle size of 0.15-4.75 mm.
6. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The recycled coarse aggregate is Class III and above recycled coarse aggregate specified in GB / T25177-2010; the recycled fine aggregate is Class III and above recycled fine aggregate specified in GB / T25176-2010.
7. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The cement is P.042.5 Portland cement.
8. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The wollastonite has a SiO2 content of ≥95% and a specific surface area of ≥20m 2 / g, loss on ignition ≤1.51%.
9. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to claim 1, characterized in that: The slag powder is S105 grade slag powder, and the loss on ignition is ≤1.0%.
10. The recycled coarse and fine aggregate concrete resistant to chloride ion corrosion according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: (1) Adding the formulated amount of recycled coarse aggregate, recycled fine aggregate, natural crushed stone and natural sand into a mixer, stirring at 75-100 rpm for 40 seconds, then adding 50% of the formulated amount of water, and stirring at 75-100 rpm for another 40 seconds to obtain an aggregate mixture; (2) The aggregate mixture is placed in a sealed container and allowed to stand for 24 hours to obtain a prepreg aggregate mixture; (3) adding all the prepreg aggregate mixture and the formulated amount of cement, silica fume, and slag powder into a mixer, stirring at 75-100 rpm for 40 seconds, then adding the formulated amount of water reducer and the remaining water, and stirring at 75-100 rpm for another 40 seconds to obtain a concrete mixture; (4) Place the concrete mixture into the mold and vibrate it on a vibration table for 20 seconds; (5) placing the concrete mixture obtained in step (4) in a cool place indoors and leaving it to stand for 24 hours; (6) After demolding, the concrete mixture of step (5) is moved into a standard curing room for curing for 28 days to obtain recycled coarse and fine aggregate concrete resistant to chloride ion corrosion. The curing temperature is 20±2° C. and the curing relative humidity is 93±3%.