Large-flow micro-expansion quick-setting tunnel blast hole blocking material and preparation method thereof

By preparing large-flow micro-expanded fast condensation tunnel gun hole blocking material, and using high-flow mortar to effectively block the gun hole, the problem of poor clogging effect in traditional construction is solved, and more efficient blasting effect and environmental protection are achieved.

CN119059773APending Publication Date: 2024-12-03JIANGHAN UNIVERSITY +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411206283.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The blasting effect of the gun holes in traditional tunnel blasting construction is not ideal, resulting in waste of blasting energy and environmental pollution, and it is difficult to achieve efficient rock breaking effect.

Method used

The preparation method of large-flow micro-expanded rapid condensation tunnel gun hole blocking material is adopted. By mixing sand, expanded cement, expansion agent, rapid condensation agent and polymer water-absorbing resin and other materials, a high-flow mortar is formed, and after filling it with the gun hole, it is Leave it in order to achieve effective blockage and improve the blasting effect.

Benefits of technology

It improves the blasting effect, extends the action time of the explosive gas, enhances the energy utilization rate of explosives, reduces the use of explosives and environmental pollution, and reduces construction costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059773A_ABST
    Figure CN119059773A_ABST
Patent Text Reader

Abstract

The invention discloses a large-flow micro-expansion quick-setting tunnel blast hole blocking material which is prepared by the following steps: mixing sand, expansive cement, an expanding agent and an accelerator in proportion, then mixing with water, a water reducing agent and high-molecular water-absorbent resin to obtain a mortar material, then filling a blast hole with the mortar material, and standing to obtain the blast hole blocking material. Compared with the prior art, the prepared blast hole blocking material has the advantages that the blasting effect is improved, the energy utilization rate of explosives is increased, and the usage amount of the explosives is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering blasting materials, and in particular to a large-flow micro-expansion fast-setting tunnel blasthole plugging material and a preparation method thereof. Background Art

[0002] As the environment of railway tunnel construction continues to change, the construction terrain and construction conditions are becoming more severe and complex, especially in areas with many mountains, the difficulty of tunnel construction is increasing, and the construction requirements are becoming higher and higher. As an important means to improve the blasting effect, blasthole plugging is widely used in the blasting field. The role of blasthole plugs is to limit the premature leakage of explosive gas in the blasthole and prolong the action time of explosive gas in the blasthole, thereby increasing the time of blasthole pressure and stress in the rock mass, and increasing the range of rock crushing. In the process of tunnel drilling and blasting construction, it is necessary not only to meet the basic construction requirements of rock fracture and crushing, but also to reduce the use of explosives as much as possible, improve the energy utilization rate of explosives, reduce harmful effects, and reduce construction costs, so as to achieve the goal of fine blasting.

[0003] In the traditional tunnel blasting construction process, due to the construction progress requirements and environmental conditions, the blastholes are usually not blocked or directly blocked with waste paper shells. Due to the unsatisfactory blocking effect, a large amount of energy is wasted in the blasting process, the role of the explosive gas is not fully utilized, and the harmful effects such as flying rocks and dust in the working area are increased, which wastes explosives and has a negative impact on the environment. Therefore, to achieve good blasting quality, reasonable blocking of blastholes plays an important role.

[0004] Therefore, how to provide a large-flow micro-expansion fast-setting tunnel blasthole plugging material so that it can maximize the role of the explosive gas in the process of plugging the blasthole and achieve the technical effect of effective blasting is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In view of the problems existing in the prior art, the technical problem to be solved by the present invention is to provide a large-flow micro-expansion fast-setting tunnel blast hole plugging material, so that it can maximize the role of explosive gas in the process of plugging the blast hole and achieve the technical effect of effective blasting.

[0006] To achieve the above-mentioned purpose, the present invention provides a method for preparing a flowing micro-expansion fast-setting tunnel blasthole plugging material, and the preparation method of the tunnel blasthole plugging material comprises: S1, adding sand, expansive cement, an expansive agent and an accelerating setting agent into a mixer, and then stirring in the mixer to obtain a mixture; S2, adding water and a water reducing agent to the mixture obtained in S1, and then stirring in the mixer, adding a polymer water-absorbing resin during the stirring process, and continuing to stir in the mixer after the polymer water-absorbing resin is completely added to obtain a mortar; S3, filling the mortar obtained in S2 into the blasthole, letting it stand, and obtaining the blasthole plugging material.

[0007] In the first aspect, the mass ratio of the S1 medium sand, expansive cement, expansive agent and accelerating agent is (0.5-1.5):(0.5-1.5):(0.035-0.105):(0.025-0.075)

[0008] In the first aspect, the mass ratio of water, water reducing agent and high molecular water-absorbing resin in S2 is (0.25-0.75):(0.025-0.075):(0.003-0.105); the mass ratio of expansive cement in S1 to water in S2 is (0.5-1.5):(0.25-0.75).

[0009] In the first aspect, the conditions for stirring in the stirrer in S1 are: the stirring time is 1 to 2 minutes; the rotation speed of the mixer of the stirrer is 57 to 67 rpm; the rotation speed of the stirring blade of the stirrer is 135 to 145 rpm; the rotation direction of the mixer of the stirrer is opposite to that of the stirring blade of the stirrer.

[0010] In the first aspect, the conditions for stirring in the mixer in S2 are: the rotation speed of the mixer of the mixer is 115-135 rpm, the rotation speed of the stirring blade of the mixer is 275-295 rpm, and the rotation direction of the mixer of the mixer is opposite to that of the stirring blade of the mixer; the conditions for continuing stirring in the mixer in S2 are: the stirring time is 1-2 minutes, the rotation speed of the mixer of the mixer is 115-135 rpm, the rotation speed of the stirring blade of the mixer is 275-295 rpm, and the rotation direction of the mixer of the mixer is opposite to that of the stirring blade of the mixer.

[0011] In the first aspect, the addition rate of the polymer water-absorbing resin in S2 is 0.5 g / min to 3 g / min.

[0012] In the first aspect, the standing time is 45 to 90 minutes; the standing temperature is 20°C to 30°C.

[0013] In the first aspect, the sand is ordinary river sand; the expansive cement is R·SAC42.5 early strength micro-expansive cement; the expansive agent is UEA-H anti-cracking expansive agent; the accelerator is CLZ type accelerator; and the water reducer is liquid polycarboxylic acid high-efficiency water reducer.

[0014] In the first aspect, the polymer water-absorbing resin is a polymer water-absorbing resin prepared using acrylic acid and sodium hydroxide as raw materials.

[0015] The present invention also provides a large flow micro-expansion fast-setting tunnel blasthole plugging material, which is prepared by the above-mentioned method for preparing a large flow micro-expansion fast-setting tunnel blasthole plugging material.

[0016] Beneficial effects:

[0017] The invention obtains a mixture by mixing sand, expansive cement, an expansive agent and an accelerator, so that the sand, the expansive cement, the expansive agent and the accelerator are in complete contact with each other; then, water and a water reducing agent are added to the mixture for stirring, and a high molecular water-absorbing resin is slowly added during the stirring process, and the addition of the water reducing agent reduces the water consumption of the mortar and improves the fluidity of the mortar, so that it is more convenient and effective to fill the blasthole in the subsequent use process; since the high molecular water-absorbing resin has a high expansion multiple, it cannot be guaranteed to be completely dispersed if added together, and it is easy to form small pieces and cannot be fully combined with water, so the high molecular water-absorbing resin is added during the stirring process, and stirring is performed while adding, so that the high molecular water-absorbing resin is evenly mixed in the mortar, and the added high molecular water-absorbing resin has strong water absorption, and its volume will expand greatly in a short time after absorbing water, and when the mortar is filled into the blasthole In the end, the polymer water-absorbing resin expands significantly, prompting the mortar material to expand as well, thereby improving the blocking effect of the mortar and reducing the amount of other materials. At the same time, during the blasting operation, the mutual friction between the blasthole blocking material and the blasthole wall after the mortar solidifies is significantly greater than the friction generated by the traditional plugging material. The plugging material fits tightly against the hole wall, making it more difficult for the explosive gas to rush out of the blasthole, extending the action time of the explosive gas, and allowing the explosive to fully react in the blasthole, thereby obtaining more sufficient explosion energy to act on the hole wall to form cracks, thereby generating a gas wedge effect, improving the rock breaking effect, and improving the working environment. After the mortar is filled into the blasthole, it needs to be left to stand for a period of time to allow the mortar to solidify. The waiting time for solidification can be the time for the connection of the detonation network to the pre-blasting preparation work, making full use of the time for the pre-blasting preparation work.In the present invention, the quick-setting agent is in the mortar material, which can make the mortar material set quickly. Therefore, the mortar material is filled into the blast hole. Since the mortar material can set quickly in the blast hole, and the quick-setting agent can enhance the mechanical strength of the mortar in the early stage, the mortar material has a certain weight, which avoids the clogging effect of the mortar on the blast hole due to the weak mechanical strength of the mortar or the light weight; at the same time, the quick-setting agent enhances the mechanical strength of the mortar in the early stage, and can increase the duration of the explosive gas in the blast hole during tunnel blasting, so that the explosive can fully react in the blast hole, thereby obtaining more sufficient explosion energy to act on the hole wall to form cracks, thereby generating a gas wedge effect and improving the rock breaking effect. In addition, the mortar material sets quickly, which can avoid extending the parallel operation time of the blasting network connection and the pre-blasting preparation work due to too long a static time; in addition, the expansion agent and expansion cement added to the mortar material, because the expansion agent and expansion cement have the function of compensating for the shrinkage and cracking of the material during the hardening process of the material, and can make the material Slight expansion occurs. After the expansion agent is added to the mortar with the expansion cement as the plugging material and filled into the blasthole, the expansion agent and the expansion cement begin to play a role in compensating for the shrinkage and cracking of the material. The slight expansion that occurs makes the plugging material fit with the blasthole wall, increases the friction between the plug and the blasthole wall, makes it less likely to punch holes during blasting, prolongs the time of the explosive gas in the blasthole, and improves the rock breaking effect; at the same time, the water reducing agent added to the mortar can improve the rheology and plasticity of the mortar, and reduce the shrinkage rate of the mortar after solidification, improves the operability and portability when the mortar is filled into the blasthole, and can realize automatic grouting and plugging operations when the mortar is filled into the blasthole; the blasthole plugging material of the present invention is simple and convenient to make, has low raw material cost, is easy to purchase, and has wide storage conditions; the blasthole plugging material of the present invention can improve the blasting effect, improve the energy utilization rate of the explosive, reduce the amount of explosive used, reduce the engineering cost, reduce the generation of harmful effects, and has important engineering application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 The present invention is a simplified process flow chart of the preparation process of the large-flow micro-expansion fast-setting tunnel blasthole plugging material. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of this specification are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of this specification, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in this specification belong to the scope of protection of the present invention.

[0021] Embodiment 1

[0022] like Figure 1 As shown, this embodiment 1 provides a method for preparing a large-flow, micro-expansion, fast-setting tunnel blasthole plugging material, and the method for preparing the tunnel blasthole plugging material includes: S1, adding sand, expansive cement, expansive agent and quick-setting agent into a mixer, and then stirring in the mixer to obtain a mixture: S2, adding water and a water reducer to the mixture obtained in S1, and then stirring in the mixer, adding a polymer water-absorbing resin during the stirring process, and after the polymer water-absorbing resin is completely added, continuing to stir in the mixer to obtain a mortar; S3, filling the mortar obtained in S2 into the blasthole, letting it stand, and obtaining the blasthole plugging material.

[0023] The invention obtains a mixture by mixing sand, expansive cement, an expansive agent and an accelerator, so that the sand, the expansive cement, the expansive agent and the accelerator are in complete contact with each other; then, water and a water reducing agent are added to the mixture for stirring, and a high molecular water-absorbing resin is slowly added during the stirring process, and the addition of the water reducing agent reduces the water consumption of the mortar and improves the fluidity of the mortar, so that it is more convenient and effective to fill the blasthole in the subsequent use process; since the high molecular water-absorbing resin has a high expansion multiple, it cannot be guaranteed to be completely dispersed if added together, and it is easy to form small pieces and cannot be fully combined with water, so the high molecular water-absorbing resin is added during the stirring process, and stirring is performed while adding, so that the high molecular water-absorbing resin is evenly mixed in the mortar, and the added high molecular water-absorbing resin has strong water absorption, and its volume will expand greatly in a short time after absorbing water, and when the mortar is filled into the blasthole In the end, the polymer water-absorbing resin expands significantly, prompting the mortar material to expand as well, thereby improving the blocking effect of the mortar and reducing the amount of other materials. At the same time, during the blasting operation, the mutual friction between the blasthole blocking material and the blasthole wall after the mortar solidifies is significantly greater than the friction generated by the traditional plugging material. The plugging material fits tightly against the hole wall, making it more difficult for the explosive gas to rush out of the blasthole, extending the action time of the explosive gas, and allowing the explosive to fully react in the blasthole, thereby obtaining more sufficient explosion energy to act on the hole wall to form cracks, thereby generating a gas wedge effect, improving the rock breaking effect, and improving the working environment. After the mortar is filled into the blasthole, it needs to be left to stand for a period of time to allow the mortar to solidify. The waiting time for solidification can be the time for the connection of the detonation network to the pre-blasting preparation work, making full use of the time for the pre-blasting preparation work.In the present invention, the quick-setting agent is in the mortar material, which can make the mortar material set quickly. Therefore, the mortar material is filled into the blast hole. Since the mortar material can set quickly in the blast hole, and the quick-setting agent can enhance the mechanical strength of the mortar in the early stage, the mortar material has a certain weight, which avoids the clogging effect of the mortar on the blast hole due to the weak mechanical strength of the mortar or the light weight; at the same time, the quick-setting agent enhances the mechanical strength of the mortar in the early stage, and can increase the duration of the explosive gas in the blast hole during tunnel blasting, so that the explosive can fully react in the blast hole, thereby obtaining more sufficient explosion energy to act on the hole wall to form cracks, thereby generating a gas wedge effect and improving the rock breaking effect. In addition, the mortar material sets quickly, which can avoid extending the parallel operation time of the blasting network connection and the pre-blasting preparation work due to too long a static time; in addition, the expansion agent and expansion cement added to the mortar material, because the expansion agent and expansion cement have the function of compensating for the shrinkage and cracking of the material during the hardening process of the material, and can make the material Slight expansion occurs. After the expansion agent is added to the mortar with the expansion cement as the plugging material and filled into the blasthole, the expansion agent and the expansion cement begin to play a role in compensating for the shrinkage and cracking of the material. The slight expansion that occurs makes the plugging material fit with the blasthole wall, increases the friction between the plug and the blasthole wall, makes it less likely to punch holes during blasting, prolongs the time of the explosive gas in the blasthole, and improves the rock breaking effect; at the same time, the water reducing agent added to the mortar can improve the rheology and plasticity of the mortar, and reduce the shrinkage rate of the mortar after solidification, improves the operability and portability when the mortar is filled into the blasthole, and can realize automatic grouting and plugging operations when the mortar is filled into the blasthole; the blasthole plugging material of the present invention is simple and convenient to make, has low raw material cost, is easy to purchase, and has wide storage conditions; the blasthole plugging material of the present invention can improve the blasting effect, improve the energy utilization rate of the explosive, reduce the amount of explosive used, reduce the engineering cost, reduce the generation of harmful effects, and has important engineering application value.

[0024] In some possible implementations, the mass ratio of the sand, expansive cement, expansive agent and accelerator in S1 is (0.5-1.5):(0.5-1.5):(0.035-0.105):(0.025-0.075).

[0025] Specifically, sand, expansive cement, expansive agent and accelerator are mixed in the above-mentioned proportion, and the mixing makes the sand, expansive cement, expansive agent and accelerator contact with each other completely. Within this proportion range, the expansion property of the mortar material can be effectively improved and the setting time can be reduced.

[0026] In some possible implementations, the mass ratio of water, water reducing agent and high molecular water-absorbing resin in S2 is (0.25-0.75):(0.025-0.075):(0.003-0.105); the mass ratio of expansive cement in S1 to water in S2 is (0.5-1.5):(0.25-0.75).

[0027] Specifically, within this ratio range, the expansion property of the obtained mortar can be effectively improved, so that the contact with the wall of the blasthole after filling is more complete, thereby improving the blasting effect, and at the same time effectively improving the rheological properties of the mortar and enhancing the operability of the mortar.

[0028] In some possible implementations, the conditions for stirring in the blender in S1 are: the stirring time is 1 to 2 minutes; the rotation speed of the mixer of the blender is 57 to 67 rpm; the rotation speed of the stirring blade of the blender is 135 to 145 rpm; the rotation directions of the mixer of the blender and the stirring blade of the blender are opposite.

[0029] Specifically, the mixer and the stirring blades of the mixer rotate in opposite directions in the mixer, so that the materials in the mixer can be stirred more completely. At the same time, when the mixer and the stirring blades rotate simultaneously, the sand, expansive cement, expansive agent and accelerator are in contact with each other and mixed completely.

[0030] In some possible implementations, the condition for then stirring in the blender in S2 is: the rotation speed of the mixer of the blender is 115-135 rpm, the rotation speed of the stirring blade of the blender is 275-295 rpm, and the rotation direction of the mixer of the blender is opposite to that of the stirring blade of the blender; the condition for continuing stirring in the blender in S2 is: the stirring time is 1-2 minutes, the rotation speed of the mixer of the blender is 115-135 rpm, the rotation speed of the stirring blade of the blender is 275-295 rpm, and the rotation direction of the mixer of the blender is opposite to that of the stirring blade of the blender.

[0031] Specifically, during the stirring process after mixing water and water reducing agent, due to the water absorption and expansion characteristics of the high molecular weight water absorbent resin, in order to ensure that the high molecular weight water absorbent resin is in complete contact with other raw materials in the mortar, the high molecular weight water absorbent resin is added while stirring to avoid the problem of mortar agglomeration and inability to disperse and uneven water absorption.

[0032] In some possible implementations, the addition rate of the polymer water-absorbing resin in S2 is 0.5 g / min to 3 g / min.

[0033] Specifically, since the polymer water-absorbent resin has strong water absorption and high expansion ratio, it cannot be guaranteed to be completely dispersed if added together, forming small pieces that cannot fully combine with water. Therefore, the polymer water-absorbent resin is added slowly to allow the polymer water-absorbent resin and water to be fully mixed to improve the expansion of the polymer water-absorbent resin.

[0034] In some possible implementations, the standing time is 45 to 90 minutes; and the standing temperature is 20°C to 30°C.

[0035] Specifically, the static time is the time for the blasting network connection and pre-blasting preparation, making full use of the time at the construction site or test.

[0036] In some possible implementations, the sand is ordinary river sand; the expansive cement is R·SAC42.5 early-strength micro-expansive cement; the expansive agent is UEA-H anti-cracking expansive agent; the accelerator is CLZ type accelerator; the water reducer is a liquid polycarboxylic acid high-efficiency water reducer; and the polymer water-absorbing resin is a polymer water-absorbing resin prepared using acrylic acid and sodium hydroxide as raw materials.

[0037] Specifically, the smaller the particle size of the sand, the larger the contact area with water, expansion agent, expansion cement, accelerator, water reducer and polymer water-absorbent resin, and the better the mechanical properties and rheological properties of the resulting blast hole plugging material; the greater the centrifugal water retention rate of the polymer water-absorbent resin, the greater the expansion of the polymer water-absorbent resin after absorbing water in a short period of time, so that the resulting mortar expands after being filled into the blast hole, reducing the use of other raw materials in the mortar, and increasing the friction between the blast hole plugging material and the blast hole wall after solidification.

[0038] Embodiment 2

[0039] Embodiment 2 of the present invention provides a large-flow micro-expansion fast-setting tunnel blasthole plugging material, which is prepared by the preparation method in the above-mentioned embodiment 1. Therefore, the performance principle of the large-flow micro-expansion fast-setting tunnel blasthole plugging material is not repeated here, and the undetailed part can be referred to embodiment 1.

[0040] In order to further illustrate the technical solution of the present application in detail to support the technical problem to be solved by the present application, the preparation method is described below with specific examples, such as Examples 1 and 2.

[0041] raw material:

[0042] Ordinary river sand: fineness modulus is 2.3~3, particle size is 0.25~0.5 mm.

[0043] High molecular water-absorbent resin: particle size is 0.083-0.122 mm; number of holes is 120-180 meshes; centrifugal water retention rate is 30g / g; pressurized absorption capacity is 15g / g.

[0044] Example 1

[0045] 800 g of ordinary river sand, 800 g of R·SAC42.5 early strength micro-expansive cement, 56 g of UEA-H anti-cracking expansion agent and 40 g of CLZ type accelerating agent were added into a JJ-15 expansive cement mortar mixer, and then stirred for 2 minutes at a mixer rotation speed of 62 rpm and a stirring blade rotation speed of 140 rpm in the JJ-15 expansive cement mortar mixer to obtain a mixture:

[0046] 400 g of water and 3.5 g of liquid polycarboxylic acid high-efficiency water reducing agent were added to the obtained mixture, and then the mixture was stirred in a JJ-15 expansive cement mortar mixer at a mixer rotation speed of 125 rpm and a stirring blade rotation speed of 285 rpm. During the stirring process, 5.6 g of a high molecular water-absorbent resin was added at a speed of 2 g / min. After the high molecular water-absorbent resin was completely added, the mixture was continued to be stirred in the JJ-15 expansive cement mortar mixer at a mixer rotation speed of 125 rpm and a stirring blade rotation speed of 285 rpm for 2 minutes to obtain a mortar material;

[0047] The obtained mortar material was filled into the blast hole, and allowed to stand at 25° C. for 60 minutes to obtain the blast hole plugging material.

[0048] Example 2

[0049] 800 g of ordinary river sand, 800 g of R·SAC42.5 early strength micro-expansive cement, 56 g of UEA-H anti-cracking expansion agent and 40 g of CLZ type accelerating agent were added into a JJ-15 expansive cement mortar mixer, and then stirred for 2 minutes at a mixer rotation speed of 62 rpm and a stirring blade rotation speed of 140 rpm in the JJ-15 expansive cement mortar mixer to obtain a mixture:

[0050] 400 g of water and 3.5 g of liquid polycarboxylate high-efficiency water reducing agent were added to the obtained mixture, and then stirred in a JJ-15 expansive cement mortar mixer at a mixer rotation speed of 125 rpm and a stirring blade rotation speed of 285 rpm for 4.8 minutes to obtain a mortar material;

[0051] The obtained mortar material was filled into the blast hole, and allowed to stand at 25° C. for 60 minutes to obtain the blast hole plugging material.

[0052] The performance tests of the mortar prepared by Examples 1-2 are as follows:

[0053] Setting time test:

[0054] Referring to the industry construction standard JGJ / T70-2009 "Test Method for Basic Performance of Building Mortar", the mortar materials obtained in Example 1 and Example 2 were respectively loaded into two penetration resistance meter barrels with a diameter of 75mm and a height of 140mm, and smoothed at a distance of 10mm from the upper plane of the penetration resistance meter barrel. Then, the penetration resistance meter barrel was placed on the pressure gauge seat of the mortar setting time measuring instrument to carry out the mortar setting time performance test. The penetration resistance value was measured repeatedly for 10 minutes. When the penetration resistance value reached 0.3MPa, the measurement was changed to once every 5 minutes until the penetration resistance value obtained by the test reached 0.7MPa. The time when the penetration resistance value reached 0.5MPa was the setting time of the mortar. The setting time of each example was tested twice. The test results of the two times are shown in Table 1. The final setting time was the average of the two times.

[0055] Table 1 Coagulation time test data

[0056] Example First test coagulation time / min Second test coagulation time / min Average value / min Example 1 28 29 28.5 Example 2 36.5 34 35.25

[0057] Mechanical properties test:

[0058] The mortars obtained in Example 1 and Example 2 were respectively loaded into two steel molds with a size of 40 mm × 40 mm × 160 mm. The steel molds were then placed on a vibration table and vibrated for 20 seconds, and then cured at 25°C for 2 hours to obtain samples with a size of 40 mm × 40 mm × 160 mm. The compressive strength and flexural strength of the samples were then tested using a cement mortar compression and flexural all-in-one machine. The test results are shown in Table 2.

[0059] Table 2 Mechanical properties test data

[0060]

[0061]

[0062] Liquidity test:

[0063] While ensuring that the freshly mixed mortar does not segregate, the mortars obtained in Example 1 and Example 2 are respectively poured into two slump barrels with a size of 50mm×100mm×150mm. The slump barrel is placed centrally on the concrete slump expansion flow meter. The slump barrel is quickly lifted up to a height of 15cm within 3 seconds. After the mortar stops flowing, the maximum diameter of the expanded circle and the diameter of the maximum diameter in the vertical direction are tested. The larger the average value of the maximum diameter of the circle and the diameter of the maximum diameter in the vertical direction, the better the fluidity of the mortar. The maximum diameter of the circle obtained by the test is 480mm, and the maximum diameter of the circle obtained in the vertical direction is 440mm, and the average value is 460mm.

[0064] Table 3 Fluidity test data

[0065] Example Maximum diameter of circle / mm Maximum diameter in vertical direction / mm Average value / mm Example 1 480 440 460 Example 2 540 430 470

[0066] Expansion test:

[0067] The expansion properties of the mortars obtained in Example 1 and Example 2 were tested using a static strain tester. A PVC pipe with a pore size of 50 mm and a height of 100 mm was selected as a filling container during the mortar test. A strain gauge was attached to the periphery of the PVC pipe. The mortar was filled into the PVC pipe and sealed so that the PVC pipe was in a horizontal state. The annular expansion force of the mortar within 2 hours was tested. The test results are shown in Table 4.

[0068] Table 4 Expansion test data

[0069] Example Expansion / με Example 1 206.42 Example 2 175.9

[0070] It can be seen from Tables 1 to 4 that the first setting time of the mortar prepared in Example 1 is 28 minutes, and the second setting time is 29 minutes. The errors of the two tests are within a reasonable range, and the average value is 28.5 minutes as the setting time of the mortar of the present invention, that is, the mortar has been set 28.5 minutes after being filled into the blasthole, which greatly shortens the time for obtaining the blasthole plugging material. The average setting time of the mortar prepared in Example 2 is 35.25 minutes, which is significantly longer than that of Example 1. The mechanical properties of the samples obtained using the mortar show that the compressive strength of Example 1 is 5.35 MPa, and the flexural strength is 1.67 MPa, and the mechanical properties are good, while the compressive strength of Example 2 is 1.92 MPa, and the flexural strength is 0 .33MPa, which is significantly lower than that of Example 1, indicating that the mechanical properties of the blasthole plugging material obtained by the mortar of Example 1 are better. In the process of blasting after plugging the blasthole, the plugging effect of the blasthole is enhanced, the time of the explosive gas in the blasthole is prolonged, the blasting effect is improved, and the occurrence of harmful effects such as flying stones in the working area is reduced. In the fluidity test of the mortars of Examples 1 and 2, the slump test average of the mortar of Example 1 is 460mm, which is significantly improved compared with the slump test average of 50-100mm of ordinary concrete mortar. At the same time, the slump test average of Example 1 is 10mm lower than the slump test average of Example 2, which is 470mm, and the error is not large, but the slump test of Example 2 is The maximum diameter of the circle is very different from the diameter in the vertical direction of the maximum diameter, which shows that the overall uniformity and consistency of the mortar in Example 2 are poor, unlike the mortar in Example 1 which has good fluidity and good uniformity and consistency. It can be seen that the addition of the polymer water-absorbing resin in the mortar improves the uniformity and consistency of the mortar, which can enhance the mechanical properties of the blasthole plugging material, and avoid the harmful effects of flying stones, dust, etc. in the working area due to the low mechanical strength of the blasthole plugging material during the blasting process. At the same time, the improvement of the uniformity and consistency of the mortar also makes the expansion of the blasthole plugging material more uniform, making the plugging of the blasthole more effective, thereby improving the blasting effect. In the expansion test, the mortar of Example 1 was filled within 2 hours. While compensating for its own contraction, it slightly expands, with an expansion of 206.42με, while the expansion of Example 2 is 175.9με. The expansion of Example 1 is significantly higher than that of Example 1, which shows that the polymer water-absorbing resin expands during the solidification process of the mortar material, and the blasthole is sealed more tightly, so that the friction between the blasthole plugging material and the blasthole wall is stronger, thereby improving the blasting effect; in summary, the present invention has a short setting time, strong fluidity, high initial strength and micro-expansion, is easy to operate and has a low cost. As a tunnel blasthole plugging material, it can improve the blasting effect, improve the energy utilization rate of explosives, reduce the amount of explosives used, reduce engineering costs, and reduce the generation of harmful effects while ensuring normal construction operations, and has important engineering application value.

[0071] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a large-flow micro-expansion fast-setting tunnel blasthole plugging material, characterized in that: The preparation method of the tunnel blasthole plugging material comprises: S1. Add sand, expansive cement, expansive agent and accelerating agent into a mixer, and then stir in the mixer to obtain a mixture: S2, adding water and a water reducing agent to the mixture obtained in S1, and then stirring in a mixer, adding a high molecular water-absorbing resin during the stirring process, and continuing to stir in the mixer after the high molecular water-absorbing resin is completely added to obtain a mortar material; S3. Fill the mortar obtained in S2 into the blast hole, let it stand, and obtain the blast hole plugging material.

2. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 1, characterized in that: The mass ratio of the S1 medium sand, expansive cement, expansive agent and accelerator is (0.5-1.5):(0.5-1.5):(0.035-0.105):(0.025-0.075).

3. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 2, characterized in that: The mass ratio of water, water reducing agent and high molecular water-absorbing resin in the S2 is (0.25-0.75):(0.025-0.075):(0.003-0.105); the mass ratio of the expansive cement in the S1 to the water in the S2 is (0.5-1.5):(0.25-0.75).

4. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 3, characterized in that: The stirring conditions in the stirrer in S1 are: the stirring time is 1 to 2 minutes; the rotation speed of the mixer of the stirrer is 57 to 67 rpm; the rotation speed of the stirring blade of the stirrer is 135 to 145 rpm; the rotation direction of the mixer of the stirrer is opposite to that of the stirring blade of the stirrer.

5. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 4, characterized in that: The conditions for stirring in the stirrer in S2 are: the rotation speed of the mixer of the stirrer is 115-135 rpm, the rotation speed of the stirring blade of the stirrer is 275-295 rpm, and the rotation directions of the mixer of the stirrer and the stirring blade of the stirrer are opposite; the conditions for continuing stirring in the stirrer in S2 are: the stirring time is 1-2 minutes, the rotation speed of the mixer of the stirrer is 115-135 rpm, the rotation speed of the stirring blade of the stirrer is 275-295 rpm, and the rotation directions of the mixer of the stirrer and the stirring blade of the stirrer are opposite.

6. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 5, characterized in that: The addition rate of the polymer water-absorbing resin in S2 is 0.5 g / min to 3 g / min.

7. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 6, characterized in that: The standing time is 45 to 90 minutes; the standing temperature is 20° C. to 30° C.

8. The large-flow micro-expansion fast-setting tunnel blasthole plugging material according to claim 7, characterized in that: The sand is ordinary river sand; the expansive cement is R·SAC42.5 early strength micro-expansive cement; the expansive agent is UEA-H anti-cracking expansive agent; the accelerator is CLZ type accelerator; and the water reducer is liquid polycarboxylic acid high-efficiency water reducer.

9. A high-flow micro-expansion fast-setting tunnel blasthole plugging material as claimed in claim 8, characterized in that: The polymer water-absorbing resin is a polymer water-absorbing resin prepared by using acrylic acid and sodium hydroxide as raw materials.

10. A high-flow micro-expansion fast-setting tunnel blasthole plugging material, characterized in that: The large flow micro-expansion fast-setting tunnel blasthole plugging material is prepared by any one of the preparation methods of a large flow micro-expansion fast-setting tunnel blasthole plugging material as described in claims 1 to 9.

Citation Information

Cited By

  • Clay-containing cement-based environment-friendly mixture and method for sealing gas drill hole by using same

    CN120364995A