Cement paste composition, cement paste as well as preparation method and application of cement paste

By combining G-level oil well cement, active materials, nanooxide and other components in the cement slurry, a cement slurry with salt resistance and strong interfacial cementation performance is solved, and the interface cementation between cement slurry and salt layer in the salt cavity gas storage is solved. The problem of poor performance improves cementing quality and seal integrity, and is suitable for frequent injection and production conditions of salt hole gas storage.

CN119059778AInactive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310635237.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cementing performance of the existing cement slurry with the salt layer in the cementing well of the salt cavity gas storage is poor, making it difficult to ensure the integrity of the wellbore and the safe and efficient operation of the gas storage.

Method used

The combination of G-grade oil well cement, active materials, nano-oxides, toughening materials, anti-salt water loss agents, low-temperature early strength agents, dispersants, defoaming agents and expansion agents is used to slurry through sodium chloride solution to form Cement slurry with salt resistance, elasticity, high premature strength and strong interface cementing properties.

Benefits of technology

It improves the cementing quality of the salt layer section, enhances the seal integrity of the cement ring, is suitable for frequent injection and production conditions of salt hole gas storage, extends the service life of the cement ring, and ensures the safe and efficient operation of the gas storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004260156960000171
    Figure BDA0004260156960000171
Patent Text Reader

Abstract

The invention discloses a cement paste composition, cement paste as well as a preparation method and application of the cement paste. The cement paste composition comprises the following components in parts by weight: 60-90 parts of G-grade oil well cement, 10-40 parts of an active material, 3-12 parts of a toughening material, 3-12 parts of nano oxide, 1-6 parts of a salt-resistant fluid loss agent, 0.5-3 parts of a low-temperature early strength agent, 0.1-1 part of a dispersing agent, 0.2-1 part of a defoaming agent, 0.5-5 parts of an expanding agent and 40-48 parts of a sodium chloride solution, wherein the 3-day activity index of the active material is 150 to 200 percent. The well cementation cement paste provided by the invention can meet the well cementation construction requirements of a salt cavern type gas storage, has the characteristics of salt resistance, high early strength, high elasticity and toughness and the like compared with conventional well cementation cement paste, and can improve the well cementation quality of a salt bed section and guarantee the sealing integrity of a cement sheath under frequent injection and production. The cement paste composition disclosed by the invention is suitable for well cementation of the salt-cavern gas storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil and gas field cementing, and in particular to a cement slurry composition, cement slurry, and a preparation method and application thereof. Background Art

[0002] There are four main types of underground gas storage, namely oil and gas reservoir type, salt cavern type, aquifer type and mine type. Among them, salt cavern gas storage has the advantages of strong peak-shaving capacity, flexibility and efficiency, and its construction scale has gradually increased in recent years. The construction of salt cavern gas storage requires drilling into the salt layer, and the dissolution of the salt layer during cementing seriously affects the cementing quality; the injection and production rounds of salt cavern gas storage far exceed those of gas reservoir type gas storage, and the sealing integrity of the cement ring under multiple rounds of strong injection and production alternating stress faces huge challenges, which puts forward strict requirements on the performance of cement slurry for cementing. Therefore, in order to improve the cementing quality of salt cavern gas storage and meet the sealing integrity of the cement ring under strong injection and production, it is necessary to develop a salt-resistant elastic and tough micro-expansion cement slurry system.

[0003] CN105906248A discloses a low-temperature, early-strength, and salt-resistant cementing slurry system. The system is prepared by using G-grade oil well cement and low-temperature, salt-resistant fluid loss agent, composite early strength agent, hollow glass microspheres, dispersant, microsilicon and other admixtures, and using 15% salt water to improve the low-temperature, early-strength performance and salt resistance. CN106244124A discloses a salt-resistant, high-density, early-strength, and anti-channeling oil well cement slurry. The system is prepared by using G-grade oil well cement, ultrafine cement, and iron ore powder, microsilicon, manganese ore powder, styrene-butadiene latex anti-channeling agent, expansion agent, fluid loss agent, retarder, dispersant, defoaming agent and other admixtures, and using 15.3wt% NaCl solution to improve the sedimentation stability of the slurry and the early strength of the cement stone, and has a strong anti-gas channeling ability.

[0004] CN113548838A discloses a freshwater salt-resistant tough cement slurry system for gas storage. The system uses fresh water to mix G-grade oil well cement with salt-resistant fluid loss reducer, salt-resistant coagulant, expansion agent, elastic agent, fiber, dispersant and other additives, thereby improving the salt resistance of the cement slurry system, increasing the early strength, and ensuring that the cement stone performance meets the strength and the influence of subsequent alternating stress.

[0005] Although the low-temperature early strength and salt resistance are improved by adding a certain concentration of salt water and accelerators to the cement slurry, and the brittleness of the cement slurry is improved by adding elastic agents, fibers and other additives for slurry preparation, the cement stone performance meets the strength and subsequent alternating stress. However, when meeting the requirements of salt resistance and elastic toughness, the interface bonding performance between the cement sheath and the salt layer is poor, and the cementing quality of the salt layer section and the cap rock section, which play an important role in the integrity of the wellbore during the operation of the gas storage, is difficult to guarantee. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems in the prior art that the interface bonding performance between the cement sheath and the salt layer is poor and the cementing quality is difficult to ensure, and to provide a cement slurry composition, cement slurry and a preparation method and application thereof. The cement slurry prepared by the cement slurry composition has the characteristics of salt resistance, elastic toughness, high early strength, strong bonding and the like, which can meet the cementing quality requirements of salt cavern gas storage and the sealing integrity of the cement sheath under injection and production throughout the life cycle, thereby ensuring the safe and efficient operation of the gas storage.

[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a cement slurry composition, which comprises: 60-90 parts by weight of G-grade oil well cement, 10-40 parts by weight of active material, 3-12 parts by weight of toughening material, 3-12 parts by weight of nano oxide, 1-6 parts by weight of salt-resistant fluid loss reducer, 0.5-3 parts by weight of low-temperature early strength agent, 0.1-1 parts by weight of dispersant, 0.2-1 parts by weight of defoaming agent, 0.5-5 parts by weight of expansion agent and 40-48 parts by weight of sodium chloride solution; wherein the 3-day activity index of the active material is 150-200%.

[0008] A second aspect of the present invention provides a cement slurry, which is prepared from the aforementioned cement slurry composition.

[0009] A third aspect of the present invention provides the aforementioned cement slurry composition or use of the aforementioned cement slurry composition in cementing of a salt cavern gas storage reservoir.

[0010] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0011] (1) The cement slurry made from the cement slurry composition of the present invention has salt resistance, elastic toughness, and early strength compared to ordinary cementing cement slurry; compared to existing cement slurry, the cement slurry of the present invention also has micro-expansion and strong interface bonding.

[0012] (2) The cement slurry of the present invention meets the following requirements: the applicable temperature range is from room temperature to 90°C, and the density range is 1.85-1.95 g / cm under 21 MPa. 3 , fluidity>20cm, upper and lower density difference is 0, the cement slurry has good fluidity and stability, and the thickening time is adjustable. When the cement stone is cured for 24h, the compressive strength is>14MPa; when it is cured for 72h, the compressive strength is>24MPa, the salt rock-cement stone interface bonding strength is>1.0MPa, the linear expansion rate is>0.02%; when it is cured for 7d, the elastic modulus is<6.0GPa.

[0013] (3) The cement slurry provided by the present invention can meet the requirements of cementing construction of salt cavern gas storage. Compared with conventional cementing cement slurry, it has the characteristics of salt resistance (under semi-saturated salt water pollution, the rheology and thickening time of cement slurry are not significantly affected), high early strength (24h compressive strength>14MPa), micro expansion (initial expansion rate>0.02%), high elastic toughness (elastic modulus<6GPa), etc., which can improve the cementing quality of salt layer section and ensure the sealing integrity of cement ring under frequent injection and production. This system is suitable for cementing of salt cavern gas storage. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] A first aspect of the present invention provides a cement slurry composition, which comprises: 60-90 parts by weight of G-grade oil well cement, 10-40 parts by weight of active material, 3-12 parts by weight of toughening material, 3-12 parts by weight of nano oxide, 1-6 parts by weight of salt-resistant fluid loss reducer, 0.5-3 parts by weight of low-temperature early strength agent, 0.1-1 parts by weight of dispersant, 0.2-1 parts by weight of defoaming agent, 0.5-5 parts by weight of expansion agent and 40-48 parts by weight of sodium chloride solution; wherein the 3-day activity index of the active material is 150-200%.

[0016] The cement slurry of the present invention can synergistically improve the interface cementation by combining active materials, nano-oxides and expansion agents. The active material uses an active material with a small average particle size. After contacting with water, the hydration rate is fast, and hydration products are quickly generated in the early stage, which are attached to the surface of the salt rock layer and hinder the salt rock from dissolving in water; the large-grained crystals containing crystal water generated by the expansion agent can compensate for the shrinkage of cement during hydration, produce micro-expansion, and further improve the interface cementation; the nano-oxide can directly fill the nano-pores in the salt rock, and can also react with cement to produce volcanic ash in the later stage, further increasing the strength of the cement stone. The three work together to comprehensively improve the interface cementation performance between the cement stone and the salt rock. And by using it in combination with other components, the cement slurry has the advantages of salt resistance, elastic toughness, micro-expansion, high early strength, strong cementation, good rheology, etc., which is suitable for cementing of salt cavern gas storage reservoirs, can improve the cementing quality of the salt layer section, and ensure the sealing integrity of the cement ring under frequent injection and production.

[0017] In the present invention, the weight of the G-grade oil well cement can be 60, 65, 70, 75, 80, 85, 90 or any value in the range of any two values, preferably 70-85 weight parts; the weight of the active material can be 10, 15, 20, 25, 30, 35, 40 or any value in the range of any two values, preferably 15-40 weight parts; the weight of the toughening material can be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or any value in the range of any two values, preferably 4-10 weight parts; the weight of the nano oxide .... The weight parts can be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 and any value in the range of any two values, preferably 4-10 weight parts; the weight parts of salt-resistant fluid loss reducer can be 1, 2, 3, 4, 5, 6 and any value in the range of any two values, preferably 3-5 weight parts; the weight parts of low-temperature early strength agent can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3 and any value in the range of any two values, preferably 1-2 weight parts; the weight parts of dispersant can be 0.1 , 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1 and any two of the range of values, preferably 0.25-0.8 parts by weight; the weight parts of the defoaming agent can be 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1 and any two of the range of values. The weight parts of the expansion agent can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5 and any value in the range composed of any two numerical values, preferably 1-3 weight parts; the weight parts of the sodium chloride solution can be 40, 41, 42, 43, 44, 45, 46, 47, 48 and any value in the range composed of any two numerical values, preferably 42-46 weight parts.

[0018] In order to further improve the salt resistance, micro-expansion, strong interface bonding, elastic toughness and early strength of the cement slurry prepared from the cement slurry composition, the cement slurry composition preferably includes: 70-85 weight parts of G-grade oil well cement, 15-40 weight parts of active materials, 4-10 weight parts of toughening materials, 4-10 weight parts of nano oxides, 3-5 weight parts of salt resistance and fluid loss reducer, 1-2 weight parts of low-temperature early strength agent, 0.25-0.8 weight parts of dispersant, 0.4-0.8 weight parts of defoaming agent, 1-3 weight parts of expansion agent and 42-46 weight parts of sodium chloride solution.

[0019] The cement slurry prepared from the cement slurry composition of the present invention has salt resistance, elastic toughness and early strength compared to common cementing cement slurry; and compared to existing cement slurry, the cement slurry of the present invention also has micro-expansion and strong interface bonding.

[0020] In some embodiments of the present invention, the active material is ultrafine cement, preferably silicate cement, with a density of 3-3.15 g / cm 3 , preferably 3.05-3.10 g / cm 3 The average particle size is 3-20 μm, preferably 5-15 μm. Under this preferred value, the ultrafine cement has a fast hydration rate and will not significantly increase the consistency of the cement slurry and affect the rheology.

[0021] In some embodiments of the present invention, the ultrafine cement is ultrafine high-aluminum silicate cement, and its aluminate content is 35-50%.

[0022] In the present invention, the active material is rapidly hydrated to generate a network flocculation structure product, which hinders the dissolution of the salt layer.

[0023] In some embodiments of the present invention, the nano-oxide is a mixture of SiO2 and Al2O3, wherein the weight ratio of SiO2 to Al2O3 is 1:0.3-0.5.

[0024] In some embodiments of the present invention, the average particle size of the nano-oxide is 35-120 nm, preferably 45-100 nm.

[0025] In the present invention, nanoparticles in the nano-oxide fill the pores of the salt rock, thereby improving the interface bonding performance between the cement sheath and the salt layer.

[0026] In some embodiments of the present invention, the expansion agent is selected from MgO and / or CaSO4.

[0027] In the present invention, the large crystals containing crystal water generated by the expansion agent can compensate for the shrinkage of cement during hydration, produce micro-expansion, and further improve the interface bonding.

[0028] In some preferred embodiments of the present invention, the expansion agent is a mixture of MgO and CaSO4, wherein the weight ratio of MgO to CaSO4 is 1:1-2. The expansion agent is a composite expansion agent, wherein the calcium expansion agent quickly generates a product containing a large amount of crystal water in the early stage, expands in volume, fills the pores formed by the dissolution of the salt rock, and hinders the further dissolution of the salt rock; the magnesium expansion agent has a slow reaction rate, reacts in the later stage, generates a product containing a large amount of crystal water, further improves the interface bonding performance, and increases the strength of the cement sheath.

[0029] In some embodiments of the present invention, the toughening material is a self-repairing elastic material, and its elongation at break is not less than 330%, preferably 330%-600%; its tensile strength at break is not less than 15MPa, preferably 15-20MPa; its elastic modulus is not less than 5MPa, preferably 5-8MPa; its average particle size is 100-200μm, preferably 150-180nm. Under this preferred value, the elastic material is easily suspended in the cement slurry and does not float.

[0030] Preferably, the self-repairing elastic material is selected from styrene acrylic particles.

[0031] In the present invention, the toughening material improves the mechanical deformation capacity of cement stone, reduces the elastic modulus of cement stone, improves the brittle characteristics of cement stone, and can ensure the integrity of the cement ring under injection-production alternating stress. At the same time, once the cement ring seal fails, the elastic material in the cement ring expands when exposed to natural gas and can repair microcracks, so that the cement ring regains its integrity.

[0032] In the present invention, G-grade oil well cement is a basic cement with a wide range of applications, and can meet the needs of cementing of almost all well types. The present invention has no special restrictions on the source of the oil well cement, and the oil well cement can be purchased from the market, such as Jiahua G-grade, Gezhouba G-grade or Yaowangshan G-grade oil well cement.

[0033] In some embodiments of the present invention, the average particle size of the G-grade oil well cement is 3-80 μm, preferably 5-75 μm, and more preferably 8-70 μm. Under this preferred value, the cement hydration rate is moderate, and the thickening time and rheology are easy to adjust.

[0034] In some embodiments of the present invention, the salt-resistant fluid loss agent is selected from one or more of 2-acrylamide-2-methylpropanesulfonic acid polymer, ketone-aldehyde condensation polymer and polyvinyl alcohol.

[0035] In some embodiments of the present invention, the low-temperature early strength agent is selected from one or more of sodium silicate, calcium chloride and calcium sulfate.

[0036] In the present invention, the low-temperature early strength agent promotes the hydration rate of cement at low temperature and improves the strength of the cement sheath at an early stage.

[0037] In some embodiments of the present invention, the dispersant is selected from high-efficiency dispersants, such as polycarboxylic acid dispersants.

[0038] In the present invention, the dispersant is preferably a high-efficiency dispersant, which has good dispersing effect and high water reduction rate of 12%-25%, or greatly increases the rheological properties of cement slurry when the water-cement ratio remains unchanged. The dispersant can depolymerize and disperse the aggregated cement particles in the cement slurry, release free water, improve the fluidity of the cement slurry, and avoid thixotropy that affects cementing construction.

[0039] In some embodiments of the present invention, the defoaming agent is selected from one or more of polyether defoaming agents, polysiloxanes and polyether-modified silicone oils.

[0040] In some embodiments of the present invention, the sodium chloride solution is a semi-saturated sodium chloride solution, and the concentration of NaCl in the semi-saturated sodium chloride solution is 18 wt %.

[0041] A second aspect of the present invention provides a cement slurry, which is prepared from the aforementioned cement slurry composition.

[0042] The performance of the cement slurry of the present invention meets the following requirements: the applicable temperature range is from room temperature to 90°C, and the density range is 1.85-1.95 g / cm under 21 MPa. 3 The cement slurry has good fluidity and stability, and the thickening time is adjustable. When the cement paste is cured for 24 hours, the compressive strength is greater than 14MPa; when it is cured for 72 hours, the compressive strength is greater than 24MPa, the salt rock-cement paste interface bonding strength is greater than 1.0MPa, and the linear expansion rate is greater than 0.02%; when it is cured for 7 days, the elastic modulus is less than 6.0GPa.

[0043] The present invention has no special limitation on the preparation method of cement slurry. The various components in the cement slurry composition described in the first aspect above can be mixed according to their weight proportions.

[0044] Specifically, the preparation method of cement slurry includes the following steps: mixing powders evenly to obtain a powder mixture, mixing liquids with additives and salt evenly to obtain a liquid mixture; and then mixing the obtained powder mixture and liquid mixture evenly to obtain cement slurry.

[0045] A third aspect of the present invention provides the aforementioned cement slurry composition or use of the aforementioned cement slurry composition in cementing of a salt cavern gas storage reservoir.

[0046] The cement slurry provided by the present invention can meet the requirements of cementing construction of salt cavern gas storage. Compared with conventional cementing cement slurry, it has the characteristics of salt resistance, high early strength, slight expansion, high elastic toughness, etc., which can improve the cementing quality of salt layer sections and ensure the sealing integrity of cement ring under frequent injection and production. The cement slurry solves the problems of poor cementing quality and annular pressure after several injection and production cycles in the prior art in such well applications.

[0047] The present invention will be described in detail below through examples.

[0048] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0049] The raw materials used in the following examples of the present invention are all commercially available products:

[0050] Grade G cement is Grade G oil well cement produced by Sichuan Jiahua Cement Plant.

[0051] The active material is the ultrafine high-alumina silicate cement produced by Sichuan Jiahua Cement Plant.

[0052] The nano-oxide is a silicon-aluminum mixed nano-material produced by Texas Continental Shelf Petroleum Engineering Technology Co., Ltd., and its model is SCYG-3 product.

[0053] The dispersant is a polycarboxylic acid dispersant produced by Texas Continental Shelf Petroleum Engineering Technology Co., Ltd., model SCF-90L.

[0054] The toughening material is the self-repairing elastic particles of Texas Continental Shelf Petroleum Engineering Technology Co., Ltd., model SCT product.

[0055] The expansion agent is a magnesium and calcium mixed expansion agent produced by Texas Continental Shelf Petroleum Engineering Technology Co., Ltd., model DZX-1 product.

[0056] The defoaming agent is a product of model DZX-1 produced by Texas Continental Shelf Petroleum Engineering Technology Co., Ltd.

[0057] The anti-salinity fluid loss agent is a product of model DZJ-Y produced by Dezhou Continental Shelf Petroleum Engineering Technology Co., Ltd.

[0058] The early strength agent is a sodium silicate early strength agent produced by Texas Continental Shelf Petroleum Engineering Technology Co., Ltd., model DZC-3 product.

[0059] Example 1

[0060] 85 parts by weight of G-grade oil well cement, 15 parts by weight of active material, 8 parts by weight of toughening material, and 3 parts by weight of expansion agent (the weight ratio of MgO and CaSO4 is 1:2) are uniformly mixed to obtain a mixture; 6 parts by weight of nano oxide (a mixture of SiO2 and Al2O3, the weight ratio is 1:0.4), 3 parts by weight of salt-resistant fluid loss reducer, 1 part by weight of low-temperature early strength agent, 0.25 parts by weight of high-efficiency polycarboxylic acid dispersant, 0.25 parts by weight of defoamer and 47.2 parts by weight of semi-saturated sodium chloride solution are mixed to obtain slurry water; the slurry water and the above mixture are stirred and mixed in a high-speed stirrer at a speed of 4000 rpm to obtain a slurry with a density of 1.93 g / cm 3 The cementing cement slurry system J-1 has a fluidity of 22 cm, a water extraction amount of 28 mL, and an upper and lower density difference of 0. The density, fluidity, water extraction amount, and upper and lower density difference of the obtained cementing cement slurry system are all measured at 25° C. and normal pressure.

[0061] The cementing cement slurry system J-1 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-1.

[0062] After testing, the 24h compressive strength of the cement paste S-1 was 21.5MPa, the 72h compressive strength was 32.2MPa, the salt rock-cement paste interface bonding strength was 1.3MPa, the linear expansion rate was 0.028%, and the 7-day elastic modulus was 5.6GPa.

[0063] Example 2

[0064] The method of Example 1 is followed, except that the amount of nano-oxide added is 10 parts by weight.

[0065] The fluidity of the cementing slurry system J-2 obtained in this example is 20 cm, the water extraction volume is 24 mL, and the upper and lower density difference is 0.

[0066] The cementing cement slurry system J-2 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-2.

[0067] After testing, the 24h compressive strength of the cement paste S-2 was 19.2MPa, the 72h compressive strength was 27.2MPa, the salt rock-cement paste interface bonding strength was 1.5MPa, the linear expansion rate was 0.027%, and the 7-day elastic modulus was 5.7GPa.

[0068] Example 3

[0069] The method of Example 1 is followed, except that the amount of nano-oxide added is 3 parts by weight.

[0070] The fluidity of the cementing slurry system J-3 obtained in this example is 23 cm, the water extraction volume is 29 mL, and the upper and lower density difference is 0.

[0071] The cementing cement slurry system J-3 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-3.

[0072] After testing, the 24h compressive strength of the cement stone S-3 was 17.1MPa, the 72h compressive strength was 25.7MPa, the salt rock-cement stone interface bonding strength was 1.1MPa, the linear expansion rate was 0.029%, and the 7-day elastic modulus was 5.5GPa.

[0073] Example 4

[0074] The method of Example 1 is followed, except that the amount of toughening material added is 10 parts by weight.

[0075] The fluidity of the cementing slurry system J-4 obtained in this example is 21 cm, the water extraction volume is 33 mL, and the upper and lower density difference is 0.

[0076] The cementing cement slurry system J-4 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-4.

[0077] After testing, the 24h compressive strength of the cement stone S-4 was 15.3MPa, the 72h compressive strength was 24.6MPa, the salt rock-cement stone interface bonding strength was 1.3MPa, the linear expansion rate was 0.032%, and the 7-day elastic modulus was 5.3GPa.

[0078] Example 5

[0079] The method of Example 1 is followed, except that the amount of toughening material added is 4 parts by weight.

[0080] The fluidity of the cementing slurry system J-5 obtained in this example is 23 cm, the water extraction volume is 23 mL, and the upper and lower density difference is 0.

[0081] The cementing cement slurry system J-5 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-5.

[0082] After testing, the 24h compressive strength of the cement stone S-5 was 23.1MPa, the 72h compressive strength was 34.3MPa, the salt rock-cement stone interface bonding strength was 1.3MPa, the linear expansion rate was 0.024%, and the 7-day elastic modulus was 5.9GPa.

[0083] Example 6

[0084] The method of Example 1 is followed, except that the amount of active material added is 35 parts by weight.

[0085] The fluidity of the cementing slurry system J-6 obtained in this example is 19 cm, the water extraction volume is 22 mL, and the upper and lower density difference is 0.

[0086] The cementing cement slurry system J-6 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-6.

[0087] After testing, the 24h compressive strength of the cement stone S-6 is 25.7MPa, the 72h compressive strength is 36.2MPa, the salt rock-cement stone interface bonding strength is 1.5MPa, the linear expansion rate is 0.023%, and the 7-day elastic modulus is 5.8GPa.

[0088] Example 7

[0089] The method of Example 1 is followed, except that the amount of active material added is 10 parts by weight.

[0090] The fluidity of the cementing slurry system J-7 obtained in this example is 23 cm, the water extraction volume is 30 mL, and the upper and lower density difference is 0.

[0091] The cementing cement slurry system J-7 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-7.

[0092] After testing, the 24h compressive strength of the cement stone S-7 is 16.2MPa, the 72h compressive strength is 27.6MPa, the salt rock-cement stone interface bonding strength is 1.2MPa, the linear expansion rate is 0.029%, and the 7-day elastic modulus is 5.5GPa.

[0093] Example 8

[0094] The method of Example 1 is followed, except that the amount of the expansion agent added is 5 parts by weight.

[0095] The fluidity of the cementing slurry system J-8 obtained in this example is 22 cm, the water extraction volume is 28 mL, and the upper and lower density difference is 0.

[0096] The cementing cement slurry system J-8 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-8.

[0097] After testing, the 24h compressive strength of the cement stone S-8 is 23.2MPa, the 72h compressive strength is 34.7MPa, the salt rock-cement stone interface bonding strength is 1.5MPa, the linear expansion rate is 0.037%, and the 7-day elastic modulus is 5.8GPa.

[0098] Example 9

[0099] The method of Example 1 is followed, except that the amount of the expansion agent added is 0.5 parts by weight.

[0100] The fluidity of the cementing slurry system J-9 obtained in this example is 22 cm, the water extraction volume is 28 mL, and the upper and lower density difference is 0.

[0101] The cementing cement slurry system J-9 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-9.

[0102] After testing, the 24h compressive strength of the cement stone S-9 is 19.7MPa, the 72h compressive strength is 31.3MPa, the salt rock-cement stone interface bonding strength is 1.0MPa, the linear expansion rate is 0.021%, and the 7-day elastic modulus is 5.5GPa.

[0103] Example 10

[0104] The method of Example 1 is followed, except that the amount of low-temperature early strength agent added is 3 parts by weight.

[0105] The fluidity of the cementing slurry system J-10 obtained in this example is 22 cm, the water extraction volume is 27 mL, and the upper and lower density difference is 0.

[0106] The cementing cement slurry system J-10 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-10.

[0107] After testing, the 24h compressive strength of the cement stone S-10 was 26.2MPa, the 72h compressive strength was 33.8MPa, the salt rock-cement stone interface bonding strength was 1.3MPa, the linear expansion rate was 0.027%, and the 7-day elastic modulus was 5.6GPa.

[0108] Embodiment 11

[0109] The method of Example 1 is followed, except that the amount of low-temperature early strength agent added is 0.5 parts by weight.

[0110] The fluidity of the cementing slurry system J-11 obtained in this example is 22 cm, the water extraction volume is 29 mL, and the upper and lower density difference is 0.

[0111] The cementing cement slurry system J-11 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-11.

[0112] After testing, the 24h compressive strength of the cement stone S-11 was 15.7MPa, the 72h compressive strength was 29.3MPa, the salt rock-cement stone interface bonding strength was 1.3MPa, the linear expansion rate was 0.029%, and the 7-day elastic modulus was 5.6GPa.

[0113] Example 12

[0114] The method of Example 1 is different in that the nano-oxide is SiO2.

[0115] The fluidity of the cementing slurry system J-12 obtained in this example is 21 cm, the water extraction volume is 35 mL, and the upper and lower density difference is 0.

[0116] The cementing cement slurry system J-12 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-12.

[0117] After testing, the 24h compressive strength of the cement stone S-12 is 15.6MPa, the 72h compressive strength is 23.9MPa, the salt rock-cement stone interface bonding strength is 1.1MPa, the linear expansion rate is 0.027%, and the 7-day elastic modulus is 5.6GPa.

[0118] Embodiment 13

[0119] The method of Example 1 is followed, except that the expansion agent is MgO.

[0120] The fluidity of the cementing slurry system J-13 obtained in this example is 21 cm, the water extraction volume is 41 mL, and the upper and lower density difference is 0.

[0121] The cementing cement slurry system J-13 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-14.

[0122] After testing, the 24h compressive strength of the cement stone S-14 was 15.3MPa, the 72h compressive strength was 24.1MPa, the salt rock-cement stone interface bonding strength was 1.0MPa, the linear expansion rate was 0.013%, and the 7-day elastic modulus was 5.6GPa.

[0123] Embodiment 14

[0124] The method of Example 1 is followed, except that the expansion agent is CaSO4.

[0125] The fluidity of the cementing slurry system J-14 obtained in this example is 19 cm, the water extraction volume is 38 mL, and the upper and lower density difference is 0.

[0126] The cementing cement slurry system J-14 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-14.

[0127] After testing, the 24h compressive strength of the cement stone S-10 was 17.8MPa, the 72h compressive strength was 26.4MPa, the salt rock-cement stone interface bonding strength was 1.0MPa, the linear expansion rate was 0.012%, and the 7-day elastic modulus was 5.6GPa.

[0128] Comparative Example 1

[0129] 100 parts by weight of G-grade oil well cement, 3 parts by weight of anti-salt fluid loss agent, 41 parts by weight of water, 0.25 parts by weight of defoamer and 47.2 parts by weight of semi-saturated sodium chloride solution were mixed to obtain a density of 1.94 g / cm 3 The cementing cement slurry system J-15 has a fluidity of 22 cm, a water separation volume of 41 mL, and a density difference of 0.

[0130] The cementing cement slurry system J-15 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-15.

[0131] After testing, the 24h compressive strength of the cement stone S-15 is 12.4MPa, the 72h compressive strength is 23.9MPa, the salt rock-cement stone interface bonding strength is 0.3MPa, the linear expansion rate is -0.004%, and the 7-day elastic modulus is 10.9GPa.

[0132] Comparative Example 2

[0133] The method of Example 1 is followed except that no nano oxide is added, and the density is 1.93 g / cm 3 The cementing cement slurry system J-16 has a fluidity of 22 cm, a water separation volume of 39 mL, and an upper and lower density difference of 0.

[0134] The cementing cement slurry system J-16 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-16.

[0135] After testing, the 24h compressive strength of the cement stone S-16 is 19.7MPa, the 72h compressive strength is 28.8MPa, the salt rock-cement stone interface bonding strength is 0.7MPa, the linear expansion rate is 0.028%, and the 7-day elastic modulus is 5.6GPa.

[0136] Comparative Example 3

[0137] The method of Example 1 was followed except that no active material was added to obtain a density of 1.93 g / cm 3 The cementing cement slurry system J-17 has a fluidity of 23 cm, a water separation volume of 32 mL, and an upper and lower density difference of 0.

[0138] The cementing cement slurry system J-17 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-17.

[0139] After testing, the 24h compressive strength of the cement stone S-17 is 12.4MPa, the 72h compressive strength is 26.5MPa, the salt rock-cement stone interface bonding strength is 0.6MPa, the linear expansion rate is 0.028%, and the 7-day elastic modulus is 5.6GPa.

[0140] Comparative Example 4

[0141] The method of Example 1 was followed except that no expansion agent was added to obtain a density of 1.93 g / cm 3 The cementing cement slurry system J-18 has a fluidity of 22 cm, a water separation volume of 28 mL, and an upper and lower density difference of 0.

[0142] The cementing cement slurry system J-18 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-18.

[0143] After testing, the 24h compressive strength of the cement stone S-18 is 20.5MPa, the 72h compressive strength is 31.4MPa, the salt rock-cement stone interface bonding strength is 0.7MPa, the linear expansion rate is -0.003%, and the 7-day elastic modulus is 5.6GPa.

[0144] Comparative Example 5

[0145] The method of Example 1 is followed, except that no toughening material is added to obtain a cementing cement slurry system J-19 with a density of 1.94 g / cm3. The cementing cement slurry system J-19 has a fluidity of 24 cm, a water extraction volume of 21 mL, and a density difference of 0.

[0146] The cementing cement slurry system J-19 and the salt rock-cement slurry assembly obtained above were cured at 60° C. for 24 h, 72 h and 7 days to obtain cement paste S-19.

[0147] After testing, the 24h compressive strength of the cement stone S-19 was 22.9MPa, the 72h compressive strength was 34.1MPa, the salt rock-cement stone interface bonding strength was 1.3MPa, the linear expansion rate was 0.026%, and the 7-day elastic modulus was 10.8GPa.

[0148] The data of the above examples and comparative examples are listed in Table 1.

[0149] Table 1

[0150]

[0151] It can be seen from the results in Table 1 that, compared with the conventional cement stone of Comparative Example 1, the elastic toughness of the cement stone obtained by Examples 1-14 is significantly increased, the interface bonding strength with the salt rock is greatly improved, the early compressive strength is increased, and the expansion rate is relatively large; Comparative Example 2 does not add nano-oxides, and the interface bonding strength between the obtained cement stone and the salt rock is relatively small; Comparative Example 3 does not add toughening materials, and the obtained cement stone has a high elastic modulus and poor elastic toughness; Comparative Example 4 does not add active materials, and the obtained cement stone has low early strength and low bonding strength; Comparative Example 5 does not add expansion agent, and the obtained cement stone shrinks, which reduces the interface bonding strength to a certain extent.

[0152] In summary, the cement slurry of the present invention, by combining active materials, nano-oxides and expansion agents with other components, can make the cement slurry have the advantages of salt resistance, elastic toughness, micro-expansion, high early strength, strong bonding, good rheology, etc., which is suitable for cementing of salt cavern gas storage, can improve the cementing quality of salt layer sections, and ensure the sealing integrity of cement ring under frequent injection and production.

[0153] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A cement slurry composition, characterized in that: The cement slurry composition comprises: 60-90 parts by weight of G-grade oil well cement, 10-40 parts by weight of active material, 3-12 parts by weight of toughening material, 3-12 parts by weight of nano oxide, 1-6 parts by weight of salt-resistant fluid loss reducer, 0.5-3 parts by weight of low-temperature early strength agent, 0.1-1 parts by weight of dispersant, 0.2-1 parts by weight of defoamer, 0.5-5 parts by weight of expansion agent and 40-48 parts by weight of sodium chloride solution; wherein the 3-day activity index of the active material is 150-200%.

2. The cement slurry composition according to claim 1, wherein The active material is ultrafine cement, with a density of 3-3.15 g / cm 3 , the average particle size is 3-20μm; Preferably, the ultrafine cement is ultrafine high-aluminum silicate cement, and its aluminate content is 35-50%.

3. The cement slurry composition according to claim 1 or 2, wherein: The nano oxide is a mixture of SiO2 and Al2O3, wherein the weight ratio of SiO2 to Al2O3 is 1:0.3-0.5; Preferably, the average particle size of the nano-oxide is 35-120 nm.

4. The cement slurry composition according to any one of claims 1 to 3, wherein: The expansion agent is selected from MgO and / or CaSO4; Preferably, the expansion agent is a mixture of MgO and CaSO4, wherein the weight ratio of MgO to CaSO4 is 1:1-2.

5. The cement slurry composition according to any one of claims 1 to 4, wherein: The toughening material is a self-repairing elastic material with a breaking elongation of 330%-600%, a breaking tensile strength of 15-20MPa, an elastic modulus of 5-8MPa, and an average particle size of 100-200μm; Preferably, the self-repairing elastic material is selected from styrene acrylic particles.

6. The cement slurry composition according to any one of claims 1 to 5, wherein: The particle size of the G-grade oil well cement is 3-80 μm.

7. The cement slurry composition according to any one of claims 1 to 6, wherein: The salt-resistant fluid loss reducer is selected from one or more of 2-acrylamide-2-methylpropanesulfonic acid polymer, ketone-aldehyde condensation polymer and polyvinyl alcohol.

8. The cement slurry composition according to any one of claims 1 to 7, wherein: The low-temperature early strength agent is selected from one or more of sodium silicate, calcium chloride and calcium sulfate.

9. The cement slurry composition according to any one of claims 1 to 10, wherein: The dispersant is selected from polycarboxylic acid dispersants.

10. The cement slurry composition according to any one of claims 1 to 11, wherein: The defoamer is selected from one or more of polyether defoamers, polysiloxanes and polyether-modified silicone oils.

11. The cement slurry composition according to any one of claims 1 to 10, wherein: The sodium chloride solution is a semi-saturated sodium chloride solution; preferably, the concentration of NaCl in the semi-saturated sodium chloride solution is 18 wt %.

12. A cement slurry, prepared from the cement slurry composition according to any one of claims 1 to 11.

13. Use of the cement slurry composition according to any one of claims 1 to 11 or the cement slurry according to claim 12 in cementing of salt cavern gas storage.

Citation Information

Patent Citations

  • Anti-salt high-density early-strength anti-channeling oil well cement slurry

    CN106244124A

  • High-temperature-resistant large-temperature-difference elastic-tough cement paste system and preparation method thereof

    CN112479635A

Cited By

  • Low-temperature early-strength micro-expansion tough material for well cementation cement and preparation method thereof

    CN120271265A