Magnesium slag unfired ceramsite and preparation method thereof

Through ball milling and granulation processes of raw materials such as magnesium slag, fly ash, etc., magnesium slag-free pottery ceramids with higher density than cores on the outer wall of the ceramic grain, solving the problems of low strength and high stacking density on the burn-free pottery ceramids, realizing the Efficient resource utilization and low-cost production.

CN119059788AInactive Publication Date: 2024-12-03ZHEJIANG ZHONGJIN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411277432.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing fire-free ceramic granules have problems with large bulk density and low strength, which limits their engineering application, and the utilization rate of magnesium slag is low, resulting in waste of resources and environmental pollution.

Method used

Using raw materials such as magnesium slag, fly ash, slag and gypsum, magnesium slag is prepared through ball milling, granulation and autoclaving treatment, to control the density of the outer wall of the ceratops to be higher than the core, to form a hard protective shell, and to improve the Mechanical strength and reduce bulk density.

Benefits of technology

The high utilization rate of magnesium slag-free pottery ceratops are achieved, with small stacking density and high strength, and the cylinder pressure strength reaches 8.49~21.75MPa, which solves the problem of long preparation time for calenders and reduces production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides magnesium slag non-sintered ceramsite and a preparation method thereof, and belongs to the technical field of ceramsite preparation. The magnesium slag non-sintered ceramsite provided by the invention is of a core-shell structure, and the fly ash is utilized as a raw material for preparing the ceramsite core and the ceramsite outer wall to provide silicon and aluminum elements, and the silicon and aluminum elements are used as main active components for forming the ceramsite; the magnesium slag is used for providing silicon and calcium elements, and the utilization rate of industrial solid waste in ingredients is increased; according to the invention, gypsum is utilized to provide calcium element, hydration of active components in fly ash is promoted, and the strength of ceramsite is improved; by controlling the proportion of the raw materials, the magnesium slag non-sintered ceramsite obtained through curing can keep high mechanical performance and low stacking density. The compactness of the outer wall of the ceramsite is controlled to be higher than that of the core of the ceramsite, the outer wall of the unfired ceramsite forms a hard protective shell, the core of the ceramsite is protected, and the mechanical strength of the magnesium slag unfired ceramsite is improved; the ceramsite core has lower compactness, so that the magnesium slag unfired ceramsite has lower bulk density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramsite preparation, and in particular to magnesium slag unfired ceramsite and a preparation method thereof. Background Art

[0002] Ceramic granules are a common large-scale resource utilization method for silicate solid waste and have high added value. Compared with sintered ceramsite, unfired ceramsite has significant advantages such as low energy consumption, controllable performance and continuous strength growth. However, due to the high density of silicate solid waste itself and the evaporation of water to generate a large number of capillary structures, unfired ceramsite has common problems such as high bulk density, high water absorption and low strength. For example, Chinese patent CN 202010408662.8 discloses an unfired ceramsite and a preparation method, which uses sludge ash, coal gangue, industrial by-product gypsum and coal gasification slag as the main raw materials to prepare all-solid waste unfired ceramsite, but this method has a long curing time (7 to 28 days), and the obtained unfired ceramsite has a large bulk density. For example, Chinese patent CN 202311375262.1 discloses a coal gasification slag unfired ceramsite and its preparation method, which utilizes the low apparent density and volcanic ash activity of coal gasification slag raw materials, and adjusts the raw material ratio and the amount of alkali activator to prepare unfired ceramsite with low volume density and low water absorption, but its cylinder pressure strength is low, and the maximum can only reach 7.2MPa. Therefore, the existing unfired ceramsite has problems such as high bulk density and low strength, which limits the engineering application of unfired ceramsite.

[0003] Magnesium slag is an industrial by-product in the magnesium production process. Nearly 5.5 to 10 tons of magnesium slag can be produced per ton of magnesium. However, the comprehensive utilization rate of magnesium slag is less than 30%, resulting in waste of resources and environmental pollution. At present, magnesium slag is mainly used in the burning of silicate cement clinker, as a cement admixture, desulfurization, etc. For example, Chinese patent CN 201510125359.6 discloses a fast-hardening silicate cement and a preparation method thereof. Although magnesium slag can be used, the amount of magnesium slag added is less than 10%, and the utilization rate of magnesium slag is low. This is because although magnesium slag has a certain volcanic ash activity, it is less active than active materials such as fly ash. When magnesium slag is used, increasing the amount of magnesium slag added is not conducive to improving the performance of the product.

[0004] Therefore, how to obtain unburned ceramsite with low bulk density and high strength while improving the utilization rate of magnesium slag is a technical problem to be solved urgently in this field. Summary of the invention

[0005] The object of the present invention is to provide a magnesium slag unfired ceramsite and a preparation method thereof. The magnesium slag unfired ceramsite provided by the present invention has the characteristics of high utilization rate of magnesium slag, low bulk density and high strength.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a magnesium slag unfired ceramsite, wherein the magnesium slag unfired ceramsite comprises a ceramsite core and a ceramsite outer wall wrapped on the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0008] The raw materials for preparing the ceramsite core include solid raw materials and spheroidizing liquid;

[0009] The raw materials for preparing the ceramsite outer wall include solid raw materials;

[0010] The solid raw materials for preparing the ceramsite core and the ceramsite outer wall include, by mass content, 0-85% fly ash, 5-30% magnesium slag, 0-85% slag and 0-10% gypsum, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6-0.8.

[0011] The present invention also provides a method for preparing the magnesium slag unfired ceramsite described in the above technical solution, comprising the following steps:

[0012] (1) ball milling the solid raw material to obtain a powder;

[0013] (2) mixing the powder obtained in part of step (1) with a ball-forming liquid, and then performing a granulation step to obtain raw ball;

[0014] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1), and performing secondary granulation to obtain initial ceramsite;

[0015] (4) Pre-curing, screening, autoclaving and drying the initial ceramsite obtained in step (3) are performed in sequence to obtain magnesium slag unfired ceramsite.

[0016] Preferably, the particle size of the powder in step (1) is ≤50 μm.

[0017] Preferably, in step (2), the mass ratio of the spheroidizing liquid to the powder is 0.05-0.40:1.

[0018] Preferably, the diameter of the raw material balls in step (2) is 100 μm to 60 mm.

[0019] Preferably, the shell thickness of the initial ceramsite in step (3) is 0.2 to 1 mm.

[0020] Preferably, the pre-curing temperature in step (4) is 30 to 50° C., and the pre-curing time is 6 to 30 hours.

[0021] Preferably, the pre-curing environment humidity is 90-99% RH.

[0022] Preferably, the steam pressure of the autoclave treatment in step (4) is 0.5 to 2.5 MPa.

[0023] Preferably, the temperature of the autoclave treatment is 185-200° C., and the time of the autoclave treatment is 2-15 hours.

[0024] The invention provides a magnesium slag unfired ceramsite, which comprises a ceramsite core and a ceramsite outer wall wrapped on the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core; the raw materials for preparing the ceramsite core comprise solid raw materials and ball-forming liquid; the raw materials for preparing the ceramsite outer wall comprise solid raw materials; the solid raw materials for preparing the ceramsite core and the ceramsite outer wall comprise, by mass content, 0-85% of fly ash, 5-30% of magnesium slag, 0-85% of slag and 0-10% of gypsum, and the proportion of the raw materials satisfies a silicon-calcium ratio of 0.6-0.8. The magnesium slag unfired ceramsite provided by the present invention is a core-shell structure, and the raw materials for preparing the ceramsite core and the outer wall of the ceramsite use fly ash to provide silicon and aluminum elements as the main active components for forming the ceramsite; the present invention uses magnesium slag to provide silicon and calcium elements, which can consume solid waste magnesium slag, increase the utilization rate of industrial solid waste in the ingredients, and reduce the production cost of unfired ceramsite; the present invention uses gypsum to provide calcium elements, promote the hydration of active components in fly ash, and improve the strength of ceramsite; the present invention controls the ratio of raw materials to meet the silicon-calcium ratio of 0.6 to 0.8. Under this ratio, it can allow the magnesium slag unfired ceramsite obtained by curing to maintain higher mechanical properties and lower bulk density under a higher magnesium slag addition amount. The present invention controls the density of the outer wall of the ceramsite to be higher than the density of the ceramsite core, so that the outer wall of the unfired ceramsite forms a hard protective shell, which plays a role in protecting the ceramsite core and improving the mechanical strength of the magnesium slag unfired ceramsite; the lower density of the ceramsite core makes the magnesium slag unfired ceramsite have a lower bulk density. The results of the embodiment show that the bulk density of the magnesium slag unfired ceramsite of the present invention is 933-1185 kg / m 3 The cylinder pressure strength is 8.49~21.75MPa, with lower bulk density and higher cylinder pressure strength. DETAILED DESCRIPTION

[0025] The present invention provides a magnesium slag unfired ceramsite, wherein the magnesium slag unfired ceramsite comprises a ceramsite core and a ceramsite outer wall wrapped on the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0026] The raw materials for preparing the ceramsite core include solid raw materials and spheroidizing liquid;

[0027] The raw materials for preparing the ceramsite outer wall include solid raw materials;

[0028] The solid raw materials for preparing the ceramsite core and the ceramsite outer wall include, by mass content, 0-85% fly ash, 5-30% magnesium slag, 0-85% slag and 0-10% gypsum, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6-0.8.

[0029] The magnesium slag unfired ceramsite provided by the invention comprises a ceramsite core.

[0030] In the present invention, the solid raw material for preparing the ceramsite core includes solid raw material and spheronizing liquid.

[0031] In the present invention, the ball-forming liquid is preferably water. In the present invention, the mass ratio of the ball-forming liquid to the solid raw material is 0.05 to 0.40:1, preferably 0.1 to 0.2:1.

[0032] In the present invention, the solid raw materials for preparing the ceramsite core include, by mass content, 0-85% fly ash, 5-30% magnesium slag, 0-85% slag and 0-10% gypsum, and the ratio of the raw materials satisfies a silicon-calcium ratio of 0.6-0.8, preferably 0.6.

[0033] In the present invention, the solid raw material for preparing the ceramsite core includes fly ash with a mass content of 0 to 85%, preferably 30 to 50%. The present invention utilizes fly ash to provide silicon and aluminum as the main active ingredients for forming ceramsite.

[0034] The present invention has no special limitation on the source of the fly ash, and the fly ash that can be obtained by those skilled in the art can be used.

[0035] In the present invention, the solid raw material for preparing the ceramsite core includes magnesium slag with a mass content of 5 to 30%, preferably 20 to 25%. In the present invention, the main components of the magnesium slag are CaO and SiO2, followed by MgO and Fe2O3, and the mineral composition is mainly β-C2S and γ-C2S, which is an industrial solid waste mainly composed of hydraulic minerals. The present invention uses magnesium slag to replace silicate cement clinker to produce unfired ceramsite, which can consume solid waste magnesium slag, increase the utilization rate of industrial solid waste in the ingredients, and reduce the production cost of unfired ceramsite.

[0036] In the present invention, the magnesium slag preferably includes, by mass content, SiO2 24.19-28.77%, Al2O3 1.12-2.54%, Fe2O3 2.41-5.96%, CaO 50.31-55.76%, MgO 6.28-7.41%, f-CaO 0.48-2.87% and Cl- 0.374-0.495%; more preferably includes: SiO2 25.88-28.77%, Al2O3 1.13-2.54%, Fe2O3 4.87-5.96%, CaO 53.57-55.76%, MgO 6.28-6.61%, f-CaO 0.48-2.05% and Cl- 0.374-0.465%. The present invention adopts the above-mentioned magnesium slag, which can provide more CaO and SiO2, ensure the strength of ceramsite and increase the amount of magnesium slag. The present invention has no special limitation on the source of the magnesium slag, and any magnesium slag that can be obtained by a person skilled in the art can be used.

[0037] In the present invention, the solid raw material for preparing the ceramsite core includes slag with a mass content of 0 to 85%, preferably 10 to 43%. The present invention provides silicon and aluminum as active components for preparing magnesium slag unfired ceramsite by adding slag. The present invention has no special limitation on the source of the slag, and any slag that can be obtained by a person skilled in the art can be used.

[0038] In the present invention, the solid raw material for preparing the ceramsite core includes gypsum with a mass content of 0 to 10%, preferably 2 to 5%. The present invention uses gypsum to provide calcium elements, promotes the hydration of active components in fly ash, and improves the strength of ceramsite. In the present invention, the gypsum is preferably desulfurized gypsum. The present invention has no special restrictions on the source of the desulfurized gypsum, and conventional commercially available desulfurized gypsum can be used.

[0039] In the present invention, the ratio of the raw materials satisfies the silicon-calcium ratio of 0.6 to 0.8, preferably 0.6. The present invention can make the ceramsite have higher strength and durability by controlling the ratio of the raw materials to make the silicon-calcium ratio within the above range.

[0040] The magnesium slag unfired ceramsite provided by the present invention comprises a ceramsite outer wall wrapped around the outer surface of the ceramsite core. In the present invention, the raw material for preparing the ceramsite outer wall is the same as the raw material for preparing the ceramsite core in the above technical solution, which will not be repeated here.

[0041] In the present invention, the particle size of the magnesium slag unfired ceramsite is preferably 1.18-19 mm, more preferably 2-10 mm; the thickness of the outer wall of the magnesium slag unfired ceramsite is preferably 0.2-1 mm, more preferably 0.5-1 mm. The present invention controls the particle size of the magnesium slag unfired ceramsite and the thickness of the outer wall of the ceramsite within the above range, so that the magnesium slag unfired ceramsite has a higher mechanical strength.

[0042] The present invention also provides a method for preparing the magnesium slag unfired ceramsite described in the above technical solution, comprising the following steps:

[0043] (1) ball milling the solid raw material to obtain a powder;

[0044] (2) mixing the powder obtained in part of step (1) with a ball-forming liquid, and then performing a granulation step to obtain raw ball;

[0045] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1), and performing secondary granulation to obtain initial ceramsite;

[0046] (4) Pre-curing, screening, autoclaving and drying the initial ceramsite obtained in step (3) are performed in sequence to obtain magnesium slag unfired ceramsite.

[0047] The present invention ball-mills solid raw materials to obtain powder.

[0048] The present invention has no special limitation on the device and parameters of the ball mill. Conventional ball mill devices and parameters can be used to make the particle size of the powder reach the desired range.

[0049] In the present invention, the particle size of the powder is preferably ≤200 μm, more preferably ≤50 μm. The present invention can destroy the glass of fly ash through ball milling, increase the specific surface area of ​​solid raw materials, stimulate the activity of fly ash, magnesium slag, slag and gypsum, and evenly mix the raw materials, improve the gelling property of the mixture, and thus help increase the strength of magnesium slag unfired ceramsite.

[0050] After obtaining the powder, the present invention mixes part of the powder with a ball-forming liquid, and then performs a granulation to obtain raw material balls.

[0051] In the present invention, the ball-forming liquid is preferably water. The present invention utilizes the ball-forming liquid to bond the powder to form raw material balls.

[0052] In the present invention, the mass ratio of the spheroidizing liquid to the powder is preferably 0.05 to 0.40: 1, more preferably 0.1 to 0.25: 1. The present invention controls the mass ratio of the spheroidizing liquid to the powder within the above range, so that the powder can be made into a wet mixed material and form tiny ball cores, which provide mother cores for subsequent primary granulation to become raw material balls.

[0053] In the present invention, the method for mixing the powder with the spheroidizing liquid is preferably to mix the powder and the atomized spheroidizing liquid evenly under stirring. The spheroidizing method of the present invention using spraying atomized water is more conducive to evenly mixing the powder with the spheroidizing liquid and forming tiny spherical cores. The present invention does not specifically limit the device for mixing the powder with the spheroidizing liquid, and a conventional mixing device can be used. In an embodiment of the present invention, the mixing device is preferably a high-speed superplastic mixer.

[0054] In the present invention, the primary granulation is preferably performed by granulating the wet mixture obtained by mixing the powder with the ball-forming liquid in a granulating device. The present invention causes the wet mixture and the ball-forming liquid to roll in the granulating device through the primary granulation, and the particle size gradually increases, and finally forms qualified raw balls. In this process, fly ash, magnesium slag and gypsum are all highly hydrophilic substances, and the surface of the particles has the ability to absorb water. During granulation, an extremely thin water film is formed on the surface of the particles, and the material is adsorbed during rolling. At the same time, due to the mechanical action during rolling, the density of the raw balls is gradually increased, resulting in a certain early strength, which can reduce the breakage rate during the secondary granulation and curing process. At the same time, the microscopic pore closure is good, which is beneficial to improve the strength of the unfired ceramsite and reduce the bulk density.

[0055] The present invention has no special restrictions on the device and parameters of the primary granulation. Conventional granulation devices and parameters can be used to make the particle size of the raw material balls meet the requirements. In an embodiment of the present invention, the granulation device is preferably a disc ball making machine.

[0056] In the present invention, the particle size of the raw ball is preferably 100 μm to 60 mm, more preferably 150 μm to 37.5 mm. The particle size of the raw ball is controlled within the above range, and the obtained raw ball has a certain initial strength.

[0057] After obtaining the raw material balls, the present invention mixes the raw material balls with part of the powder material and performs secondary granulation to obtain initial ceramsite.

[0058] The present invention has no special limitation on the mass ratio of the raw material balls to the powder, and the ratio can be adjusted to achieve the desired shell thickness of the initial ceramsite.

[0059] In the present invention, the method of mixing the raw material balls with the powder is preferably carried out in the secondary granulation. In the present invention, the device of the secondary granulation is preferably a drum coating machine or a disc pelletizing machine. The present invention can wrap a shell layer on the outer surface of the raw material balls by mixing the raw material balls with the powder for secondary granulation. Since the powder is directly used for granulation, the shell layer on the surface of the initial ceramsite has a higher density than the raw material balls, and a hard shell layer is formed after curing, which is beneficial to improve the mechanical strength of the magnesium slag unfired ceramsite. The present invention does not specifically limit the parameters of the secondary granulation, and it is sufficient to make the shell layer thickness of the initial ceramsite reach the required value.

[0060] In the present invention, the shell thickness of the initial ceramsite is preferably 0.2-1 mm, more preferably 0.5-1 mm. The present invention controls the shell thickness of the initial ceramsite within the above range, which can provide the initial ceramsite with suitable mechanical strength.

[0061] After obtaining the initial ceramsite, the present invention sequentially performs pre-curing, screening, autoclaving and drying on the initial ceramsite to obtain magnesium slag unfired ceramsite.

[0062] In the present invention, the pre-curing temperature is preferably 30-50°C, more preferably 35-40°C; the pre-curing time is preferably 6-30h, more preferably 12-22h; the pre-curing environment humidity is preferably 90-99%RH, more preferably 99%RH. The present invention controls the pre-curing parameters within the above range, so that the initial ceramsite gradually hardens, and the mechanical strength of the initial ceramsite is improved. The strength of the ceramsite after pre-curing can reach 5-6MPa. The present invention does not specifically limit the pre-curing device, and a conventional curing device that can provide the above parameters can be used. In an embodiment of the present invention, the pre-curing device is preferably a constant temperature and humidity curing box.

[0063] In the present invention, the screening is preferably a double-layer screen, the size of the upper screen hole is preferably ≤19mm, and the size of the lower screen hole is preferably ≥1.18mm. The present invention can remove large and small balls to obtain balls with a particle size of 1.18-19mm by adopting the above screening method.

[0064] In the present invention, the steam pressure of the autoclave treatment is preferably 0.5-2.5MPa, more preferably 1.0-1.2MPa; the temperature of the autoclave treatment is preferably 185-200°C, more preferably 195-200°C; the time of the autoclave treatment is preferably 2-15h, more preferably 6-12h. The present invention uses autoclave treatment to quickly penetrate into the initial ceramsite and the raw material particles with the help of water vapor under pressure, so that the silicon dioxide and aluminum oxide in the raw material are dissolved quickly, and the dissolved matter reacts quickly with calcium hydroxide, while promoting the hydration reaction to proceed quickly, thereby reducing the preparation time of the unfired ceramsite and improving the strength of the product. The present invention does not specifically limit the device for the autoclave treatment, and a conventional autoclave treatment device can be used. In an embodiment of the present invention, the autoclave treatment device is preferably a high-filling vertical energy-saving reactor.

[0065] In the present invention, the drying temperature is preferably 105° C.; the present invention has no particular limitation on the drying time, as long as the autoclaved ceramsite is fully dried.

[0066] The present invention promotes fly ash, magnesium slag and gypsum to form raw material balls with certain mechanical strength through primary granulation, and then wraps a shell layer on the surface of the raw material ball through secondary granulation, so that the density of the shell layer gradually increases from the inside to the outside in the thickness direction, giving the ceramsite a hard shell layer, and after curing and autoclaving, magnesium slag unfired ceramsite with low bulk density and high cylinder pressure strength can be obtained. The method provided by the present invention is simple to operate and has a short curing time, which solves the problem of long curing time in conventional unfired ceramsite methods.

[0067] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0068] Example 1

[0069] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0070] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 78% fly ash, 20% magnesium slag and 2% gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0071] The magnesium slag has the following composition: SiO2 28.77%, Al2O3 1.12%, Fe2O3 5.96%, CaO 55.76%, MgO 6.61%, f-CaO 0.48% and Cl-0.465%;

[0072] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0073] (1) ball-milling fly ash, magnesium slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0074] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc pelletizing machine to obtain raw material balls with a particle size of 150 μm to 37.5 mm; wherein the mass ratio of water to powder is 0.1:1;

[0075] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a disc pelletizing machine, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0076] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 30° C. and the humidity to 99% RH, and pre-curing for 22 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0077] Example 2

[0078] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0079] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 78% fly ash, 20% magnesium slag and 2% desulfurized gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0080] The magnesium slag is composed of SiO2 24.19%, Al2O3 1.13%, Fe2O3 4.81%, CaO 50.31%, MgO 7.47%, f-CaO 2.87% and Cl - 0.495%;

[0081] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0082] (1) ball-milling fly ash, magnesium slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0083] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc pelletizing machine to obtain raw material balls with a particle size of 150 μm to 37.5 mm; wherein the mass ratio of water to powder is 0.1:1;

[0084] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a disc pelletizing machine, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0085] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 30° C. and the humidity to 99% RH, and pre-curing for 22 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0086] Example 3

[0087] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0088] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 78% fly ash, 20% magnesium slag and 2% gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0089] The magnesium slag is composed of SiO2 25.88%, Al2O3 2.54%, Fe2O3 2.41%, CaO 53.57%, MgO 6.28%, f-CaO 2.05% and Cl - 0.374%;

[0090] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0091] (1) ball-milling fly ash, magnesium slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0092] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc-type pelletizing machine to obtain raw material balls with a particle size of 100 μm to 60 mm; wherein the mass ratio of water to powder is 0.1:1;

[0093] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a disc pelletizing machine, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0094] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 30° C. and the humidity to 99% RH, and pre-curing for 22 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0095] Example 4

[0096] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0097] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 30% fly ash, 25% magnesium slag, 43% slag and 2% gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0098] The magnesium slag is composed of SiO2 28.77%, Al2O3 1.12%, Fe2O3 5.96%, CaO 55.76%, MgO 6.61%, f-CaO 0.48% and Cl - 0.465%;

[0099] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0100] (1) ball-milling fly ash, magnesium slag, slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0101] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc pelletizing machine to obtain raw material balls with a particle size of 100 μm to 60 mm; wherein the mass ratio of water to powder is 0.2:1;

[0102] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a pan granulator, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0103] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 50° C. and the humidity to 99% RH, and pre-curing for 12 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0104] Example 5

[0105] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0106] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 30% fly ash, 25% magnesium slag, 43% slag and 2% gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0107] The magnesium slag is composed of SiO2 24.19%, Al2O3 1.13%, Fe2O3 4.81%, CaO 50.31%, MgO 7.47%, f-CaO 2.87% and Cl - 0.495%;

[0108] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0109] (1) ball-milling fly ash, magnesium slag, slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0110] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc pelletizing machine to obtain raw material balls with a particle size of 100 μm to 60 mm; wherein the mass ratio of water to powder is 0.2:1;

[0111] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a pan granulator, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0112] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 50° C. and the humidity to 99% RH, and pre-curing for 12 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0113] Example 6

[0114] A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite consisting of a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core;

[0115] The raw materials for preparing the ceramsite core and the ceramsite outer wall are: 30% fly ash, 25% magnesium slag, 43% slag and 2% gypsum by mass content, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6;

[0116] The magnesium slag is composed of SiO2 25.88%, Al2O3 2.54%, Fe2O3 2.41%, CaO 53.57%, MgO 6.28%, f-CaO 2.05% and Cl - 0.374%;

[0117] The preparation method of the above-mentioned magnesium slag unfired ceramsite is:

[0118] (1) ball-milling fly ash, magnesium slag, slag and gypsum to obtain a powder with a particle size of ≤50 μm;

[0119] (2) the powder obtained in step (1) and the water sprayed by atomization are uniformly stirred in a stirring chamber to form a wet mixture, and then the wet mixture and the water are subjected to a primary granulation in a disc pelletizing machine to obtain raw material balls with a particle size of 100 μm to 60 mm; wherein the mass ratio of water to powder is 0.2:1;

[0120] (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1) in a disc pelletizing machine, and performing secondary granulation to obtain initial ceramsite with a shell thickness of 0.2 to 1 mm;

[0121] (4) placing the initial ceramsite obtained in step (3) in a constant temperature and humidity curing box, setting the temperature to 50° C. and the humidity to 99% RH, and pre-curing for 12 hours; then using a double-layer sieve with an upper sieve hole of 10 mm and a lower sieve hole of 5 mm to obtain ceramsite with a particle size of 5 to 10 mm, placing it in a high-filling vertical energy-saving reactor, setting the temperature to 185° C. and the pressure to 1.0 MPa, performing autoclave treatment for 4 hours, and then drying at 105° C. for 3 hours to obtain magnesium slag unfired ceramsite.

[0122] Test Example 1

[0123] The bulk density and cylinder compressive strength of the magnesium slag unfired ceramsite prepared in Examples 1 to 6 were tested according to GB / T 17431.2, and the results are shown in Table 1:

[0124] Table 1 Performance test results of magnesium slag unfired ceramsite prepared in Examples 1 to 6

[0125] <![CDATA[Bulk density (kg / m 3 )]]> Cylinder compressive strength (MPa) Example 1 933 9.38 Example 2 963 8.74 Example 3 1045 8.49 Example 4 1185 21.75 Example 5 1056 12.32 Example 6 1041 11.41

[0126] It can be seen from the above examples that the bulk density of the magnesium slag unfired ceramsite provided by the present invention is 933-1185 kg / m 3 The cylinder pressure strength is 8.49-21.75 MPa, with low bulk density and high cylinder pressure strength. In addition, from the perspective of the preparation method, the preparation time of unfired ceramsite can be greatly shortened, solving the problem of long preparation time of unfired ceramsite.

[0127] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A magnesium slag unfired ceramsite, the magnesium slag unfired ceramsite comprising a ceramsite core and a ceramsite outer wall wrapped around the outer surface of the ceramsite core; the density of the ceramsite outer wall is higher than the density of the ceramsite core; The raw materials for preparing the ceramsite core include solid raw materials and spheroidizing liquid; The raw materials for preparing the ceramsite outer wall include solid raw materials; The solid raw materials for preparing the ceramsite core and the ceramsite outer wall include, by mass content, 0-85% fly ash, 5-30% magnesium slag, 0-85% slag and 0-10% gypsum, and the ratio of the raw materials meets the silicon-calcium ratio of 0.6-0.

8.

2. The method for preparing the magnesium slag unfired ceramsite according to claim 1 comprises the following steps: (1) ball milling the solid raw material to obtain a powder; (2) mixing the powder obtained in part of step (1) with a ball-forming liquid, and then performing a granulation step to obtain raw ball; (3) mixing the raw material balls obtained in step (2) with part of the powder obtained in step (1), and performing secondary granulation to obtain initial ceramsite; (4) Pre-curing, screening, autoclaving and drying the initial ceramsite obtained in step (3) are performed in sequence to obtain magnesium slag unfired ceramsite.

3. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: The particle size of the powder in step (1) is ≤200 μm.

4. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: In the step (2), the mass ratio of the spheroidizing liquid to the powder is 0.05-0.40:

1.

5. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: The diameter of the raw material balls in step (2) is 100 μm to 60 mm.

6. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: The shell thickness of the initial ceramsite in step (3) is 0.2 to 1 mm.

7. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: The pre-curing temperature in step (4) is 30 to 50° C. and the pre-curing time is 6 to 30 hours.

8. The method for preparing magnesium slag unfired ceramsite according to claim 7, characterized in that: The pre-curing environment humidity is 90-99% RH.

9. The method for preparing magnesium slag unfired ceramsite according to claim 2, characterized in that: The steam pressure of the autoclave treatment in step (4) is 0.5 to 2.5 MPa.

10. The method for preparing magnesium slag unfired ceramsite according to claim 2 or 9, characterized in that: The temperature of the autoclave treatment is 185-200° C., and the time of the autoclave treatment is 2-15 hours.