Fluorite derived structure oxide aerogel as well as preparation method and application thereof

Through the preparation of fluorite-derived structure oxide aerogel, sol gel and high-temperature heat treatment technology, the problem of structure collapse of traditional oxide aerogels in high temperature and high radiation environments is solved, and low density and high specific surface area are achieved and low thermal conductivity, suitable for thermal insulation materials in nuclear reactors.

CN119059814AActive Publication Date: 2024-12-03HARBIN INST OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411183600.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Traditional oxide aerogels cannot maintain the integrity of the pore structure in high temperature and high radiation environments, and cannot achieve the synergistic effect of radiation resistance and high temperature heat insulation, and the high density is not suitable for the space limitations of nuclear reactors.

Method used

Using the preparation method of fluorite-derived structure oxide aerogel, the combination of rare earth elements and transition group metal elements is used to prepare low density, high specific surface area and A2B7O17 structural aerogel with low thermal conductivity.

Benefits of technology

The obtained aerogels maintain a complete macro/micromorphology under high temperature and strong radiation environments, have high stability and long-term service capabilities, and are suitable as thermal insulation materials for nuclear reactors, broadening the application prospects of oxide aerogels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059814A_ABST
    Figure CN119059814A_ABST
Patent Text Reader

Abstract

The invention relates to fluorite derived structure oxide aerogel as well as a preparation method and application thereof, and belongs to the technical field of functional materials. In order to solve the problem that the traditional oxide aerogel cannot stably serve in a high-temperature and high-radiation environment for a long time, the invention provides the fluorite derived structure oxide aerogel, the crystal structure of the aerogel is A2B7O17, A is a rare earth element, and B is a transition metal element. The aerogel is subjected to high-temperature heat treatment, the reaction activity is reduced, and pore structure collapse and volume shrinkage occurring when the aerogel is used in a high-temperature environment can be reduced; a fluorite-derived crystal structure in the aerogel can absorb neutrons in a nuclear radiation environment to keep a complete macro / micro morphology, so that the aerogel can be used as an efficient heat-insulating material in high-temperature and intense-radiation environments of a nuclear reactor with high stability and long service time, and the application of the oxide aerogel is widened; the material has a wide application prospect in the field of nuclear reactor heat insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and in particular relates to a fluorite-derived structural oxide aerogel and a preparation method and application thereof. Background Art

[0002] Thermal insulation materials play a vital safety role in nuclear reactors. They can effectively reduce the rate of heat transfer to the surrounding environment, reduce heat loss, improve energy efficiency, and protect equipment within the reactor from high temperature damage.

[0003] The internal environment of a nuclear reactor is extreme, with high temperature, high pressure and strong radiation, which places extremely high demands on the performance of thermal insulation materials. Nuclear radiation mainly affects the performance of thermal insulation materials by destroying the molecular structure of the material, causing chemical bond breakage, molecular deformation and atomic structure changes, including material embrittlement, changes in thermal conductivity, reduced fire resistance and impaired chemical stability.

[0004] Fluorite-derived structural oxides are similar to fluorite (calcium fluoride, CAF 2 ) structural characteristics, with a stable cubic structure. During the radiation process, the disordered phase structure can be maintained, which can resist radiation-induced amorphization, enhance radiation tolerance, and avoid cracking and failure of the material. β-phase fluorite-derived structured oxide ceramics are considered to be a very promising material with broad application prospects in the field of high-radioactive nuclear waste solidification.

[0005] Although fluorite-derived structural oxide ceramics can maintain structural stability at high temperatures, their thermal conductivity is relatively high. This means that in high-temperature environments such as nuclear reactors, heat may be transferred through ceramic materials relatively quickly, limiting their thermal insulation effect. Moreover, fluorite-derived structural oxide ceramics generally have higher density and larger volume. In space-constrained environments such as nuclear reactors, overly heavy insulation materials may increase the burden on the structure and reduce overall efficiency.

[0006] Aerogel is a lightweight material with abundant nanoscale pores, high specific surface area and ultra-low thermal conductivity, but common oxide aerogels are mostly SiO 2 Aerogel, Al 2 O 3 Aerogel, ZrO 2 Aerogels, etc., become single-component oxide crystals after high-temperature heat treatment. It is difficult for them to maintain a complete pore structure in a strong radiation environment, and it is impossible to achieve the coordination of radiation resistance and high-temperature thermal insulation. Summary of the invention

[0007] In order to solve the problem that traditional oxide aerogels cannot serve stably for a long time in a high temperature and high radiation environment, the present invention provides a fluorite-derived structured oxide aerogel and a preparation method and application thereof.

[0008] The technical solution of the present invention:

[0009] A fluorite-derived oxide aerogel, wherein the crystal structure of the aerogel is A 2 B 7 O 17 , where A is a rare earth element and B is a transition metal element.

[0010] Furthermore, the rare earth element is one of Y, Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu, and the transition metal element is one of Ti, Zr or Hf.

[0011] A method for preparing a fluorite-derived structural oxide aerogel, comprising the following steps:

[0012] Step 1: Prepare gel:

[0013] Adding a rare earth element precursor and a transition metal precursor to a mixed solvent of deionized water and anhydrous ethanol, stirring in a water bath to obtain a mixed solution, adding glacial acetic acid to the mixed solution, stirring in a water bath, cooling to room temperature, adding epichlorohydrin, and stirring for a certain period of time to obtain gel I;

[0014] Step 2: Aging treatment:

[0015] The gel I obtained in step 1 is immersed in anhydrous ethanol, and the anhydrous ethanol is replaced regularly until aging is completed to obtain gel II;

[0016] Step 3: Supercritical drying:

[0017] The gel II obtained in step 2 is placed in a supercritical drying device, anhydrous ethanol is added to soak the gel II, nitrogen is introduced, the temperature is increased under a certain pressure, the pressure is increased after the temperature is increased to the drying temperature, and the temperature and pressure are maintained for a certain period of time to obtain BO 2 -A 2 O 3 Composite aerogel;

[0018] Step 4: Heat treatment:

[0019] The BO obtained in step 3 2 -A 2 O 3 The composite aerogel is placed in a heat treatment device, heated to a heat treatment temperature at a certain rate, and kept at the heat treatment temperature for a certain time to obtain a fluorite-derived structure oxide aerogel.

[0020] Furthermore, in step 1, the rare earth element precursor is a nitrate hydrate of a selected rare earth element; the transition metal precursor is a tetrachloride of a transition metal; the molar ratio of the rare earth element precursor to the transition metal precursor is 1:3.5; and the concentration of the transition metal tetrachloride in the mixed solution is 10%wt.

[0021] Furthermore, in step 1, the volume ratio of the deionized water to the anhydrous ethanol is 1:10; the added amounts of the glacial acetic acid and the epichlorohydrin are calculated based on the molar ratio of the transition metal precursor, glacial acetic acid and epichlorohydrin of 1:1.5:4.

[0022] Furthermore, the water bath stirring temperature in step 1 is 40° C., the water bath stirring time is 30 min, and the stirring time after adding epichlorohydrin is 2 to 10 min.

[0023] Furthermore, in step 2, the gel I is immersed in anhydrous ethanol at an ambient temperature of 45° C., and the anhydrous ethanol is replaced regularly every 12 hours, for a total of 6 times.

[0024] Furthermore, the gas pressure during the heating in step three is 3.5 MPa, the heating rate is 4°C / min, the drying temperature is 273°C, the gas pressure is increased by increasing the nitrogen pressure to 9 MPa, and the heat and pressure holding time is 2h.

[0025] Furthermore, the heating rate in step 4 is 5-10°C / min, the heat treatment temperature is 900-1200°C, and the insulation time is 30-60min.

[0026] An application of the fluorite-derived structural oxide aerogel provided by the invention in thermal insulation of a nuclear reactor.

[0027] Beneficial effects of the present invention:

[0028] The present invention efficiently obtains an oxide aerogel with a fluorite-derived structure through sol-gel, aging, supercritical drying, and high-temperature heat treatment. The obtained aerogel has a carbon content of 0.5 g / cm 3 Density below 100m 2 / g or more specific surface area, 0.05W / (m·K) or less thermal conductivity; the macroscopic appearance is a complete block.

[0029] The aerogel in the present invention has been subjected to a high temperature heat treatment at 900-1200°C, and the reaction activity is reduced, which can reduce the pore structure collapse and volume shrinkage when used in a high temperature environment; at the same time, the present invention is a multi-component oxide aerogel, and the aerogel forms a fluorite-derived crystal structure A 2 B 7 O17, It can absorb neutrons in a nuclear radiation environment and maintain a complete macro / micro morphology. It can be used as a high-efficiency thermal insulation material with high stability and long service life in the high temperature and strong radiation environment of a nuclear reactor. It broadens the application of oxide aerogels and has broad application prospects in the field of nuclear reactor thermal insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a physical picture of the fluorite-derived structured oxide aerogel obtained in Example 1;

[0031] Figure 2 This is the XRD image of the fluorite-derived structured oxide aerogel obtained in Example 1;

[0032] Figure 3 This is a SEM image of the fluorite-derived structured oxide aerogel obtained in Example 1;

[0033] Figure 4 This is a SEM image of the fluorite-derived structured oxide aerogel obtained in Example 2;

[0034] Figure 5 This is a SEM image of the fluorite-derived structured oxide aerogel obtained in Example 3. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.

[0036] Example 1

[0037] This embodiment provides a fluorite derivative structure of Y 2 Hf 7 O 17 Oxide aerogel and preparation method thereof.

[0038] The crystal structure of the aerogel in this embodiment is Y 2 Hf 7 O 17 , the rare earth element is yttrium, and the transition metal element is hafnium.

[0039] The preparation method of the fluorite-derived structured oxide aerogel in this embodiment comprises the following steps:

[0040] Step 1: Prepare gel:

[0041] Weigh the rare earth element precursor yttrium nitrate hexahydrate Y(NO 3 ) 3 6H 2 O and transition metal precursor hafnium tetrachloride HfCl 4 , added to a mixed solvent of deionized water and anhydrous ethanol in a volume ratio of 1:10, stirred in a water bath at 40°C for 30 minutes to form a mixed solution, wherein the total concentration of yttrium nitrate hexahydrate and hafnium tetrachloride in the mixed solution is 10%wt;

[0042] According to HfCl 4 With CH 3 The molar ratio of COOH was 1:1.5. Glacial acetic acid was added to the obtained mixed solution, stirred in a water bath at 40°C for 30 min, cooled to room temperature, and heated to 40°C. 4 Epichlorohydrin was added to the mixed system cooled to room temperature at a molar ratio of 1:4, and gel I was formed after stirring for 10 minutes;

[0043] Step 2: Aging treatment:

[0044] Soak the gel I obtained in step 1 in anhydrous ethanol, place it in an environment of 45°C, replace the anhydrous ethanol every 12 hours, and replace it 6 times in total to obtain gel II;

[0045] Step 3: Supercritical drying:

[0046] The gel II obtained in step 2 was placed in a supercritical drying reactor, anhydrous ethanol was added to soak the gel II, nitrogen was introduced to maintain a pressure of 3.5 MPa, and then the temperature was raised to a drying temperature of 273°C at a heating rate of 4°C / min, the exhaust valve was adjusted to maintain a pressure of 9 MPa, and the temperature and pressure were maintained for 2 hours. The gas in the reactor was released and cooled to room temperature to obtain HfO 2 -Y 2 O 3 Composite aerogel;

[0047] Step 4: Heat treatment:

[0048] The HfO obtained in step 3 2 -Y 2 O 3 The composite aerogel was placed in a muffle furnace and heated to a heat treatment temperature of 1100°C at a heating rate of 7°C / min. After being kept at this temperature for 40 minutes, a fluorite-derived structure of Y 2 Hf 7 O 17 of oxide aerogels.

[0049] Figure 1This is a physical picture of the fluorite-derived structured oxide aerogel obtained in Example 1; the picture shows that the macroscopic appearance of the fluorite-derived structured oxide aerogel is a complete block.

[0050] Figure 2 This is the XRD picture of the fluorite-derived oxide aerogel obtained in Example 1. It can be seen that the aerogel forms a fluorite-derived crystal structure Y 2 Hf 7 O 17 , and its characteristic diffraction peak corresponds to PDF card 28-1450.

[0051] The fluorite derivative structure obtained in this embodiment is Y 2 Hf 7 O 17 The density of the oxide aerogel is 0.27 g / cm 3 , the specific surface area is 157.73m 2 / g, and its thermal conductivity is 0.027W / (m·K), which meets the requirements of lightweight and porous thermal insulation materials for nuclear reactors.

[0052] Example 2

[0053] This embodiment provides a fluorite derivative structure of Sc 2 Zr 7 O 17 Oxide aerogel and preparation method thereof.

[0054] The crystal structure of the aerogel in this embodiment is Sc 2 Zr 7 O 17 , the rare earth element is scandium, and the transition metal element is zirconium.

[0055] The preparation method of the fluorite-derived structured oxide aerogel in this embodiment comprises the following steps:

[0056] Step 1: Prepare gel:

[0057] The rare earth element precursor scandium nitrate hexahydrate (Sc(NO)) was weighed according to a molar ratio of 1:3.5. 3 ) 3 6H 2 O and transition metal precursor zirconium tetrachloride ZrCl 4 , added to a mixed solvent of deionized water and anhydrous ethanol in a volume ratio of 1:10, stirred in a water bath at 40°C for 30 minutes to form a mixed solution, wherein the total concentration of scandium nitrate hexahydrate and zirconium tetrachloride in the mixed solution is 10%wt;

[0058] According to ZrCl 4 With CH 3The molar ratio of COOH was 1:1.5. Glacial acetic acid was added to the obtained mixed solution, stirred in a water bath at 40°C for 30 min, cooled to room temperature, and then heated to 40°C. 4 Epichlorohydrin was added to the mixed system cooled to room temperature at a molar ratio of 1:4, and gel I was formed after stirring for 10 minutes;

[0059] Step 2: Aging treatment:

[0060] Soak the gel I obtained in step 1 in anhydrous ethanol, place it in an environment of 45°C, replace the anhydrous ethanol every 12 hours, and replace it 6 times in total to obtain gel II;

[0061] Step 3: Supercritical drying:

[0062] The gel II obtained in step 2 was placed in a supercritical drying reactor, anhydrous ethanol was added to soak the gel II, nitrogen was introduced to maintain a pressure of 3.5 MPa, and then the temperature was raised to a drying temperature of 273°C at a heating rate of 4°C / min, the exhaust valve was adjusted to maintain a pressure of 9 MPa, and the temperature and pressure were maintained for 2 hours. The gas in the reactor was released and cooled to room temperature to obtain ZrO 2 -Sc 2 O 3 Composite aerogel;

[0063] Step 4: Heat treatment:

[0064] The ZrO obtained in step 3 2 -Sc 2 O 3 The composite aerogel was placed in a muffle furnace and heated to a heat treatment temperature of 1000°C at a heating rate of 5°C / min. After being kept at this temperature for 30 minutes, a fluorite-derived structure of Sc was obtained. 2 Zr 7 O 17 of oxide aerogels.

[0065] The fluorite derivative structure obtained in this embodiment is Sc 2 Zr 7 O 17 The density of the oxide aerogel is 0.31 g / cm 3 , the specific surface area is 152.64m 2 / g, and thermal conductivity is 0.034W / (m·K).

[0066] Example 3

[0067] This embodiment provides a fluorite-derived structure of La 2 Ti 7 O 17 Oxide aerogel and preparation method thereof.

[0068] The crystal structure of the aerogel in this embodiment is La 2 Ti 7 O 17 , the rare earth element is lanthanum, and the transition metal element is titanium.

[0069] The preparation method of the fluorite-derived structured oxide aerogel in this embodiment comprises the following steps:

[0070] Step 1: Prepare gel:

[0071] The rare earth element precursor lanthanum nitrate hexahydrate La(NO 3 ) 3 6H 2 O and transition metal precursor titanium tetrachloride TiCl 4 , added to a mixed solvent of deionized water and anhydrous ethanol in a volume ratio of 1:10, stirred in a water bath at 40°C for 30 minutes to form a mixed solution, wherein the total concentration of lanthanum nitrate hexahydrate and titanium tetrachloride in the mixed solution is 10%wt;

[0072] According to TiCl 4 With CH 3 The molar ratio of COOH was 1:1.5. Glacial acetic acid was added to the obtained mixed solution, stirred in a water bath at 40°C for 30 min, cooled to room temperature, and then heated to 40°C. 4 Epichlorohydrin was added to the mixed system cooled to room temperature at a molar ratio of 1:4, and gel I was formed after stirring for 10 minutes;

[0073] Step 2: Aging treatment:

[0074] Soak the gel I obtained in step 1 in anhydrous ethanol, place it in an environment of 45°C, replace the anhydrous ethanol every 12 hours, and replace it 6 times in total to obtain gel II;

[0075] Step 3: Supercritical drying:

[0076] The gel II obtained in step 2 was placed in a supercritical drying reactor, anhydrous ethanol was added to soak the gel II, nitrogen was introduced to maintain a pressure of 3.5 MPa, and then the temperature was raised to a drying temperature of 273°C at a rate of 4°C / min. The exhaust valve was adjusted to maintain a pressure of 9 MPa, and the temperature was maintained for 2 hours. The gas in the reactor was released and cooled to room temperature to obtain TiO 2 -La 2 O 3 Composite aerogel;

[0077] Step 4: Heat treatment:

[0078] The TiO obtained in step 3 2 -La2 O 3 The composite aerogel was placed in a muffle furnace and heated to a heat treatment temperature of 900°C at a heating rate of 5°C / min. After being kept at this temperature for 60 minutes, a fluorite-derived structure of La 2 Ti 7 O 17 of oxide aerogels.

[0079] The fluorite derived structure obtained in this embodiment is La 2 Ti 7 O 17 The density of the oxide aerogel is 0.33 g / cm 3 , the specific surface area is 148.72m 2 / g, and thermal conductivity is 0.038W / (m·K).

[0080] Figure 3 , Figure 4 , Figure 5 The SEM images of the fluorite-derived structured oxide aerogels obtained in Example 1, Example 2, and Example 3 respectively show that the examples prepared by the technology of the present invention have a typical rich nanoscale pore structure, which has a high specific surface area and low thermal conductivity and can effectively insulate in a high temperature environment.

Claims

1. A fluorite-derived structural oxide aerogel, characterized in that: The crystal structure of the aerogel is A2B7O 17 , where A is a rare earth element and B is a transition metal element.

2. The fluorite-derived structural oxide aerogel according to claim 1, characterized in that: The rare earth element is one of Y, Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu, and the transition metal element is one of Ti, Zr or Hf.

3. A method for preparing the fluorite-derived structured oxide aerogel according to claim 1 or 2, characterized in that: Here are the steps: Step 1: Prepare gel: Adding a rare earth element precursor and a transition metal precursor to a mixed solvent of deionized water and anhydrous ethanol, stirring in a water bath to obtain a mixed solution, adding glacial acetic acid to the mixed solution, stirring in a water bath, cooling to room temperature, adding epichlorohydrin, and stirring for a certain period of time to obtain gel I; Step 2: Aging treatment: The gel I obtained in step 1 is immersed in anhydrous ethanol, and the anhydrous ethanol is replaced regularly until aging is completed to obtain gel II; Step 3: Supercritical drying: The gel II obtained in step 2 is placed in a supercritical drying device, anhydrous ethanol is added to soak the gel II, nitrogen is introduced, the temperature is increased under a certain pressure, the pressure is increased after the temperature is increased to the drying temperature, and the temperature and pressure are maintained for a certain period of time to obtain a BO2-A2O3 composite aerogel; Step 4: Heat treatment: The BO2-A2O3 composite aerogel obtained in step 3 is placed in a heat treatment device, heated to a heat treatment temperature at a certain rate, and kept at the heat treatment temperature for a certain time to obtain a fluorite-derived structure oxide aerogel.

4. The method for preparing the fluorite-derived structured oxide aerogel according to claim 3, characterized in that: In step 1, the rare earth element precursor is a nitrate hydrate of a selected rare earth element; the transition metal precursor is a tetrachloride of a transition metal; the molar ratio of the rare earth element precursor to the transition metal precursor is 1:3.5; and the concentration of the transition metal tetrachloride in the mixed solution is 10%wt.

5. The method for preparing the fluorite-derived structured oxide aerogel according to claim 3 or 4, characterized in that: In step 1, the volume ratio of the deionized water to the anhydrous ethanol is 1:10; the added amounts of the glacial acetic acid and the epichlorohydrin are calculated based on the molar ratio of the transition metal precursor, glacial acetic acid and epichlorohydrin of 1:1.5:

4.

6. The method for preparing fluorite-derived structured oxide aerogel according to claim 5, characterized in that: The water bath stirring temperature in step 1 is 40° C., the water bath stirring time is 30 min, and the stirring time after adding epichlorohydrin is 2 to 10 min.

7. The method for preparing fluorite-derived structured oxide aerogel according to claim 6, characterized in that: In step 2, the gel I is immersed in anhydrous ethanol at an ambient temperature of 45° C., and the anhydrous ethanol is replaced regularly every 12 hours, for a total of 6 times.

8. The method for preparing fluorite-derived structured oxide aerogel according to claim 7, characterized in that: In step 3, the gas pressure during the heating is 3.5 MPa, the heating rate is 4°C / min, the drying temperature is 273°C, the gas pressure is increased by adjusting the nitrogen pressure to 9 MPa, and the heat and pressure holding time is 2h.

9. The method for preparing fluorite-derived structured oxide aerogel according to claim 8, characterized in that: The heating rate in step 4 is 5-10°C / min, the heat treatment temperature is 900-1200°C, and the insulation time is 30-60min.

10. Use of the fluorite-derived structured oxide aerogel as claimed in claim 1 or 2 in thermal insulation of a nuclear reactor.

Citation Information

Patent Citations

  • Rare-earth-based aerogel material with radiation shielding effect and heat insulation property as well as preparation and application of rare-earth-based aerogel material

    CN110563435A

  • Graphene / rare earth composite aerogel material, preparation method thereof and nuclear reactor thermal insulation material

    CN116606156A

  • Integration building green system based on rooftop rainwater bank for climate crisis adaptation

    KR102386824B1

  • In-situ aerogels and methods of making same

    US20150068974A1

  • Monolithic rare earth oxide aerogels

    US20170267925A1