Method for recycling waste polyester through acid-base concerted catalysis and methanol hydrolysis

Through the acid-base synergistic catalysis method, the synergistic effect of phenolic substances and strong alkali catalysts is used to solve the problems of harsh methanolylation reaction conditions and high catalyst costs, achieving mild degradation of PET and efficient DMT recovery, which is suitable for a variety of PETs. Samples, including colored materials.

CN119059903AActive Publication Date: 2024-12-03ZHEJIANG UNIV

Patent Information

Application Number
CN202411554004.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
2044-11-04

AI Technical Summary

Technical Problem

The existing PET methanolylation reaction conditions are harsh, the catalyst costs are high, and it may cause environmental pollution, making it difficult to achieve high yield DMT recovery under mild conditions.

Method used

The acid-base synergistic catalysis method is used, and phenolic substances are used as acid additives and strong alkali catalysts to synergize the reaction path and pH value, promote the mild degradation of PET, and form the high-value product DMT.

Benefits of technology

Efficient degradation of PET is achieved under mild conditions, improving the yield and purity of DMT, reducing energy consumption and environmental pollution, and is suitable for a variety of PET samples, including difficult-to-treat non-ferrous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an acid-base synergistic catalysis waste polyester methanolysis recovery method, which comprises the following steps: adding polyester waste plastics, an acidic auxiliary agent and a basic catalyst into methanol, and carrying out a depolymerization reaction to obtain dicarboxylic acid ester, the basic catalyst is strong alkali, acetate, phosphate, carbonate, pypocholoride, meta-aluminate, alkoxide or phenate. According to the method for directionally converting the waste polyester under the synergistic catalysis of the acid and the alkali, the rapid and mild degradation of the polyester waste plastic is successfully realized. The method not only improves the degradation efficiency, but also can obtain chemicals with high added value, and has the advantages of small pollution, strong controllability, green and cheap catalyst, low cost input and the like. In addition, a reaction system of the method is close to neutral, corrosion to equipment is low, safety and environmental protection are achieved, energy consumption is low, a brand new thought is provided for efficient waste polyester methanolysis recovery, and the method has extremely high industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of comprehensive utilization of waste resources, and in particular to a method for recovering waste polyester by methanol decomposition catalyzed by acid and base synergy. Background Art

[0002] Plastics have been widely used in modern society due to their excellent properties such as lightweight and corrosion resistance. According to statistics, the global plastic production reached 450 million tons in 2020, and it is showing an upward trend year by year. However, the widespread use of plastics has also brought severe environmental challenges. A large number of plastic products are used as disposable items and then discarded in the environment, accumulating in various ecosystems, causing the so-called "white pollution". In addition, more than 90% of the plastics currently produced are derived from fossil raw materials, which have limited reserves and are non-renewable. Due to the lack of plastic recycling and reuse, it is estimated that the economic losses caused by the disposal of plastic products are as high as more than 80 billion US dollars each year. Therefore, it has become a top priority to develop appropriate methods for the resource utilization of plastics to achieve a win-win situation of environmental and economic benefits.

[0003] Polyethylene terephthalate (PET) is one of the most widely used plastics, accounting for about 11% of the world's annual plastic production. At present, the recycling methods of waste PET plastics mainly include mechanical recycling, energy recycling and chemical recycling. The first two methods often lead to waste of resources, do not meet the requirements of sustainable development and dual carbon goals, and limit the recycling capacity of PET. In contrast, chemical recycling can effectively reduce the consumption of petroleum raw materials while producing high value-added materials. It is considered to be the most ideal recycling process and is also the focus of current research.

[0004] Chemical recycling of PET mainly includes five degradation pathways: hydrolysis, glycolysis, alcoholysis, aminolysis and ammonialysis. Among them, methanolysis has significant advantages in processing low-quality polyester bottles. It can not only process low-quality raw materials, but also its product ethylene glycol terephthalate (DMT) is easier to separate and purify. Therefore, methanolysis has become the object of extensive research and large-scale application.

[0005] In the prior art, there are many patents on PET methanolysis. For example, the patent document with publication number CN110938231A discloses "a method for the methanolysis of waste PET polyester catalyzed by low eutectic solvent". This method uses a self-synthesized urea-based low eutectic solvent as a catalyst and methanol as a solvent to alcoholyze PET to obtain a high yield of DMT; the patent document with publication number CN113735705A discloses "a method for the methanolysis of waste PET polyester catalyzed by polyionic liquid". By using polyionic liquid (such as PIL-Zn 2+ 、PIL-Co 2+ 、PIL-Mn 2+etc.) to catalyze methanolysis of waste PET polyester.

[0006] Although the above-mentioned alcoholysis catalytic system can achieve complete degradation of PET, it still has some shortcomings: some catalysts are expensive and may cause environmental pollution; the reaction conditions are harsh and energy consumption is high, the reaction temperature usually needs to reach above 170°C, and it is difficult to obtain high yields of DMT under mild conditions; the co-solvents used in some methods may bring additional environmental and safety risks. Therefore, it is urgent to develop a method that can efficiently depolymerize waste polyester and obtain high-yield, high-value products under mild methanolysis reaction conditions. This will not only help reduce environmental pollution and reduce preparation costs, but will also greatly promote the upgrading and transformation of waste polyester, and provide new technical support for the sustainable use of plastics. Summary of the invention

[0007] In order to solve the bottleneck problems of traditional PET methanolysis, such as harsh reaction conditions, high catalyst cost and environmental pollution, the present invention proposes a method for recycling waste polyester methanolysis by acid-base synergistic catalysis, which can rapidly degrade waste PET under mild conditions and prepare high-value chemical DMT in a targeted manner. The method of the present invention has a simple process flow, high economic benefits, and can achieve high-value recycling of waste polyester plastics.

[0008] A method for recovering waste polyester by methanolysis by acid-base synergistic catalysis, comprising the following steps: Polyester waste plastics, an acidic auxiliary agent and an alkaline catalyst are added to methanol to carry out a depolymerization reaction to obtain dicarboxylic acid esters, wherein the acidic auxiliary agent is a phenolic substance and the alkaline catalyst is a strong base, acetate, phosphate, carbonate, hypochlorite, aluminate, alcohol salt or phenol salt.

[0009] In the efficient depolymerization of polyester waste plastics, the acid-base synergistic catalytic mechanism is crucial. Alkaline catalysts provide hydroxide ions to attack ester bonds, reduce their stability and promote breakage, form alcohol anions, accelerate alcoholysis reactions, and adjust the pH value to improve product selectivity. However, alkaline environments may trigger side reactions, so acidic additives are introduced. Acidic additives can change the reaction path, promote proton transfer, inhibit excessive base catalysis, adjust product distribution, and synergistically improve catalytic efficiency with alkaline catalysts.

[0010] The acidic auxiliary agent of the present invention adopts phenolic substances, which ionize H⁺ ions in a high-temperature methanol solution, fine-tune the pH value of the reaction system, maintain acid-base balance, and thus optimize the catalytic efficiency. At the same time, the acidity of phenols promotes the protonation of ester bonds in polyester molecules, accelerates the alcoholysis reaction, and improves efficiency. In addition, phenolic substances can also react with unstable intermediates or by-products, inhibit the occurrence of side reactions, and improve the yield and purity of the target product. At the same time, the mild acidity of phenolic auxiliary agents reduces equipment corrosion and safety hazards, making the alcoholysis process more gentle and easy to control.

[0011] The alkaline catalyst of the present invention is selected from strong bases, acetates, phosphates, carbonates, hypochlorites, aluminates, alcoholates or phenolates, which can effectively promote the breaking of lipid bonds, maintain the acid-base balance of the reaction system, regulate the reaction process, and make the alcoholysis reaction easier to proceed.

[0012] The present invention not only optimizes the reaction path and product distribution through the acid-base synergistic effect of phenolic substances and alkaline catalysts, but also improves the reaction rate and product quality, reduces energy consumption and subsequent processing difficulty, provides strong support for the recycling of polyester waste plastics, and realizes precise control and efficient conversion of polyester molecular structure.

[0013] Preferably, the polyester waste plastic is made of polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyethylene succinate or polyethylene adipate. Before adding the polyester waste plastic into the reaction device, it needs to be pre-crushed into centimeter-level flakes, particles or powders to ensure the resource utilization effect of the waste polyester material and to obtain the dicarboxylic acid ester monomer with high yield through targeted upgrading.

[0014] More preferably, the polyester waste plastic is made of polyethylene terephthalate, including polyethylene terephthalate waste bottles, polyethylene terephthalate waste films, polyethylene terephthalate color trays, polyethylene terephthalate color ropes or polyethylene terephthalate non-woven fabrics. The method of the present invention is applicable to a variety of PET samples, including difficult-to-treat materials such as colored PET materials, and the recovery rate can be as high as 72%-96%, showing excellent efficiency and adaptability.

[0015] Preferably, the phenolic substances include at least one of guaiacol, methyl guaiacol, ethyl guaiacol, hydroquinone, pyrogallol, tannic acid, pomegranate polyphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, p-bromophenol, p-cresol, phenol, 2-ethylphenol, 4-aminophenol, dichlorophenol, trichlorophenol, pentachlorophenol, p-methoxyphenol or bisphenol A. The present invention increases the diversity of products by introducing a variety of phenolic substances to meet specific needs. At the same time, the above-mentioned phenolic substances are mostly derived from natural products or bio-based chemicals, which have better environmental compatibility than synthetic acidic additives, meet the principles of green chemistry, and reduce the impact on the environment.

[0016] Preferably, the molar ratio of the phenolic substance to the polyester waste plastic is (0.01-4):1. More preferably, the molar ratio of the phenolic substance to the polyester waste plastic is (0.05-1.5):1. Too low a molar ratio of phenolic substance to polyester waste plastic will lead to incomplete reaction and low product yield; too high a molar ratio will cause waste of resources, increase costs, and increase the difficulty of product purification. Therefore, the present invention preferably limits the molar ratio of phenolic substance to polyester waste plastic to 0.05-1.5:1, which can ensure that the phenolic substance can fully play its role and promote the full depolymerization of polyester waste plastic, and avoid unnecessary cost increase and product purification problems, while taking into account reaction efficiency and economy.

[0017] Preferably, the strong base includes at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide or calcium hydroxide. The above strong base can effectively promote the cleavage of the ester bond and accelerate the alcoholysis reaction process. At the same time, it can neutralize the acidic substances produced in the reaction, maintain the acid-base balance of the reaction system, and is conducive to the continuous progress of the reaction.

[0018] Preferably, the acetate includes at least one of lithium acetate, sodium acetate, potassium acetate, cesium acetate, calcium acetate or zinc acetate; the phosphate includes at least one of lithium phosphate, sodium phosphate, potassium phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate or cesium phosphate; the carbonate includes at least one of lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, cesium bicarbonate, lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate or magnesium carbonate. Acetates, phosphates and carbonates can ionize in solution to produce hydroxide ions, thereby showing alkalinity. When the above salts are used as catalysts, they not only have good catalytic activity, but also have relatively mild reaction conditions and are less corrosive to equipment. In addition, these salts are widely available and have low costs, which helps to reduce production costs.

[0019] Preferably, the hypochlorite comprises at least one of sodium hypochlorite or potassium hypochlorite. Hypochlorite has certain oxidizing properties, can play an auxiliary catalytic role in the alcoholysis reaction, and can inhibit the occurrence of side reactions to a certain extent, thereby improving the yield and purity of the target product.

[0020] Preferably, the aluminate includes at least one of sodium aluminate or potassium aluminate. Aluminate can form stable aluminum hydroxy complexes in solution, which have a catalytic effect on the cleavage of ester bonds and can also interact with other components in the reaction system to regulate the reaction process.

[0021] Preferably, the alkoxide includes at least one of lithium methoxide, lithium ethoxide, lithium isopropoxide, sodium methoxide, sodium ethoxide, sodium tert-butoxide, sodium propoxide, sodium isopropoxide, potassium methoxide, potassium ethoxide, potassium tert-butoxide, potassium propoxide or potassium isopropoxide; the phenolate includes at least one of sodium catechol, sodium hydroquinone, sodium resorcinol, sodium cresol, potassium phenolate or sodium phenolate. The coordination effect of the metal ions in the alkoxide and phenolate with the alcohol or phenol gives it unique catalytic performance. The above-mentioned alkoxide and phenolate have high selectivity for the alcoholysis reaction of the present invention, can effectively promote the generation of the target product, and it also has certain environmental friendliness, which is in line with the development trend of green chemistry.

[0022] Preferably, the molar ratio of the alkaline catalyst to the polyester waste plastic is (0.01-1):1. More preferably, the molar ratio of the alkaline catalyst to the polyester waste plastic is (0.05-0.3):1. Too low a catalyst dosage may lead to incomplete alcoholysis, while an excessive amount of the catalyst increases costs and environmental risks. The present invention limits the molar ratio of the alkaline catalyst to the polyester waste plastic within the above range, can efficiently catalyze the polyester alcoholysis reaction, ensure the purity and selectivity of the product, and simplify the purification process and reduce costs.

[0023] Preferably, the amount of methanol added per mmol of polyester waste plastic is 0.1~6 mL. More preferably, the amount of methanol added per mmol of polyester waste plastic is 0.5~1.5 mL. The amount of methanol added is mainly based on the consideration of reaction efficiency and product purity. Methanol is used as an alcoholysis agent, and its appropriate addition can effectively promote the decomposition of polyester, improve the reaction rate and yield. If the amount of methanol added is insufficient, the alcoholysis reaction may be incomplete, affecting the purity of the product; and if too much is added, it will not only cause waste, but also may induce side reactions and increase the difficulty of product separation. In addition, an appropriate amount of methanol also helps to control the reaction temperature, avoid local overheating, and ensure that the reaction proceeds smoothly. The present invention limits the amount of methanol added to the above range to achieve efficient and high-purity polyester alcoholysis.

[0024] Preferably, the reaction temperature of the depolymerization reaction is 60-200°C, and the reaction time is 0.5-18 h. Further preferably, the reaction temperature of the depolymerization reaction is 90-150°C, and the reaction time is 1.5-6 h. More preferably, the reaction temperature of the depolymerization reaction is 100-130°C, and the reaction time is 2-3 h. The method of the present invention controls the reaction conditions within the above range, which can inhibit the occurrence of side reactions and ensure high selectivity and yield of the target product.

[0025] Preferably, the material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is guaiacol, and the alkaline catalyst is potassium bicarbonate or cesium bicarbonate. The present invention uses guaiacol as an acidic auxiliary agent and potassium bicarbonate as an alkaline catalyst. The combination of the two provides a good acid-base balance. The mild acidity of guaiacol and the alkalinity of potassium bicarbonate synergistically promote the protonation of the ester bond and accelerate the cleavage process, thereby improving the conversion rate and product selectivity of PET alcoholysis.

[0026] Preferably, the molar ratio of polyethylene terephthalate to guaiacol, potassium bicarbonate or cesium bicarbonate is 1:(0.05-1.5):(0.05-0.3), and the amount of methanol added per mmol of polyethylene terephthalate is 0.5-1.5 mL.

[0027] Preferably, the polyester waste plastic is made of polyethylene terephthalate, the acidic auxiliary agent is methyl guaiacol, and the alkaline catalyst is potassium methoxide or potassium phenoxide. The structural difference of methyl guaiacol makes it more stable than guaiacol under certain conditions. When combined with potassium methoxide or potassium phenoxide, it can effectively control side reactions and increase the yield of alcoholysis products.

[0028] Preferably, the molar ratio of polyethylene terephthalate to methylguaiacol, potassium methoxide or potassium phenoxide is 1:(0.05-1.5):(0.05-0.3), and the amount of methanol added per mmol of polyethylene terephthalate is 0.5-1.5 mL.

[0029] Preferably, the material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is ethyl guaiacol, and the alkaline catalyst is sodium hypochlorite. The combination of ethyl guaiacol and sodium hypochlorite shows a more efficient catalytic effect when treating PET containing special pollutants, and the oxidizing property of sodium hypochlorite helps to remove certain impurities that are difficult to treat.

[0030] Preferably, the molar ratio of polyethylene terephthalate to ethyl guaiacol and sodium hypochlorite is 1:(0.05-1.5):(0.05-0.3), and the amount of methanol added per mmol of polyethylene terephthalate is 0.5-1.5 mL.

[0031] More preferably, the material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is guaiacol, the alkaline catalyst is potassium bicarbonate, the molar ratio of the polyester waste plastic to the acidic auxiliary agent and the alkaline catalyst is 1:1:0.1, and the amount of methanol added per mmol of the polyester waste plastic is 1 mL. Under the reaction conditions, the conversion rate of the polyester waste plastic is close to 100%, and the yield of the product can reach up to 99%.

[0032] In addition, the combination of the above-mentioned guaiacols and specific alkaline catalysts (guaiacol + potassium bicarbonate or cesium bicarbonate, methyl guaiacol + potassium methoxide or potassium phenolate, ethyl guaiacol + sodium hypochlorite) showed strong anti-interference ability against dyes and impurities. The mild acidity of guaiacols and the alkalinity of specific catalysts synergistically overcome the catalytic inhibition that may be caused by dyes, significantly improve the depolymerization efficiency, and show significant advantages in the treatment of colored plastics.

[0033] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention proposes an innovative acid-base synergistic catalytic directional conversion method for waste polyester, which successfully achieves the rapid and mild degradation of polyester waste plastics. This method not only improves the degradation efficiency, but also produces high value-added chemicals, opening up a new way for the resource utilization of polyester waste plastics; (2) The acid-base synergistic catalytic system used in the present invention has significant advantages in terms of environmental friendliness and economy. Taking the preferred guaiacol / potassium bicarbonate catalytic system as an example, the weak alkalinity of potassium bicarbonate greatly reduces the corrosion resistance requirements of the equipment, which is conducive to industrial application; and guaiacol as an acid auxiliary is a bio-based solvent with the characteristics of being green and low-cost, which is fully in line with the concept of sustainable development. The design of this catalytic system fully reflects the innovation of the present invention in green chemistry and industrial practice; (3) The acid-base synergistic catalytic directional conversion method of waste polyester of the present invention exhibits excellent catalytic performance, and can achieve a yield of more than 99% of ethylene glycol and a yield of more than 97% of dimethyl terephthalate. The method has a wide range of applicability and can efficiently process various types of waste PET raw materials, including but not limited to waste PET bottles, waste PET matrix films, PET colored ropes and PET non-woven fabrics. All types of PET waste can be efficiently upgraded and converted in a short period of time, significantly improving the resource utilization level and economic value of waste PET; (4) The application prospects of the present invention are not limited to PET waste plastics, but can also be extended to other polyester materials, such as polyethylene succinate (PES) and polyethylene adipate (PEA). This high adaptability greatly broadens the range of materials for waste plastic treatment. While ensuring high depolymerization efficiency, this method can also achieve rapid reaction and quickly convert various polyester materials into corresponding high-value ester products. By simply adjusting the reaction conditions, this method can flexibly cope with different types of polyester waste, fully demonstrating its great potential and universality in industrial applications, and providing new technical support for the comprehensive utilization of polyester waste plastics; (5) The method of the present invention is not only applicable to transparent plastics, but also shows good depolymerization effects on a variety of polyester wastes including colored bottle flakes. Even when faced with highly crystalline materials such as PET woven tapes, this technology can achieve high yields. The method of the present invention provides a powerful tool for processing complex polyester wastes, especially showing significant advantages in processing colored plastics. DETAILED DESCRIPTION

[0034] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description through specific embodiments. In the following description, many specific details are set forth in order to fully understand the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below. The technical features in each embodiment of the present invention can be combined accordingly without conflicting with each other.

[0035] In the following embodiments of the present invention, a method for recovering waste polyester by methanolysis by acid-base synergistic catalysis is provided, and the specific steps include: S1. Place crushed polyester materials, acidic additives, alkaline catalysts and methanol solvents in a reaction device; wherein the polyester materials are made of polyethylene terephthalate (PET), polyethylene succinate or polyethylene adipate, etc. In addition, the molar ratio of the amount of the acidic additive added to the polyester material is (0.01-4):1, the molar ratio of the amount of the alkaline catalyst added to the polyester material is (0.01-1):1, and the amount of methanol added is 0.1-6 mL / mmol of polyester material; S2. Place the above reaction device at a depolymerization temperature of 60-200℃ to carry out methanol depolymerization reaction for 0.5-18 hours. In this reaction process, based on the acid-base synergistic catalytic mechanism, polyester waste plastic methanol depolymerization is achieved under low temperature and low pressure conditions. After the above reaction is completed, it is cooled to room temperature to obtain high-value esters, realizing the high-value recycling of polyester waste plastics.

[0036] The present invention can be used for depolymerization and upgrading of waste PET materials, and can also be used for other polyesters, such as polyethylene succinate and polyethylene adipate, which are also suitable for the recycling strategy of the present invention, and the products are corresponding esters and ethylene glycol. Taking PET material as an example, the products are dimethyl terephthalate and ethylene glycol.

[0037] The application examples of the acid-base synergistic catalytic process of the present invention in common polyester waste plastics are as follows: Example 1

[0038] 3 mmol PET powder, 3 mmol guaiacol, 0.3 mmol potassium bicarbonate and 3 mL methanol were added to a pressure-resistant glass tube equipped with a stirrer, placed in an oil bath, and stirred and heated. The reaction system was heated to 120 ° C and reacted at this temperature for 6 h. After the reaction was completed, it was cooled to room temperature, and the resulting mixed solution and the precipitated solid were the products. Dichloromethane was added to dissolve, and the dissolving solution was determined by GC to determine the yield, with mesitylene as the internal standard. The results showed that the yield of ethylene glycol (EG) in this embodiment was 99.0%, and the yield of dimethyl terephthalate (DMT) was 97.2%. Embodiment 2-5

[0039] The following examples investigate the reaction temperature. The difference from Example 1 is that the reaction temperature in the methanolysis reaction conditions is changed, corresponding to Examples 2-5 respectively.

[0040] Add 3 mmol PET powder, 3 mmol guaiacol, 0.3 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system is heated to 90-150°C and reacts at this temperature for 6 h. After the reaction is completed, cool to room temperature, and the resulting mixed solution and precipitated solid are the products. Add dichloromethane to dissolve, add mesitylene as an internal standard, and the yield of EG and DMT is determined by GC in the dissolved solution. The reaction results are shown in Table 1.

[0041] Embodiment 6-8

[0042] The following examples investigate the reaction time, and the difference from Example 1 is that the reaction time in the methanolysis reaction conditions is changed, corresponding to Examples 6-8 respectively.

[0043] Add 3 mmol PET powder, 3 mmol guaiacol, 0.3 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system is heated to 120°C and reacts at this temperature for 1.5-6 hours. After the reaction is completed, cool to room temperature, and the resulting mixed solution and precipitated solid are the products. Add dichloromethane to dissolve, add mesitylene as an internal standard, and the yield of EG and DMT is determined by GC in the dissolved solution. The reaction results are shown in Table 2.

[0044] Examples 9-12

[0045] The following examples investigate the dosage of the acidic auxiliary agent. The difference from Example 1 is that the dosage of guaiacol in the methanolysis reaction conditions is changed, corresponding to Examples 9-12 respectively.

[0046] Add 3 mmol PET powder, 1.5-4.5 mmol guaiacol, 0.3 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system was heated to 120°C and reacted at this temperature for 2 h. After the reaction was completed, the temperature was lowered to room temperature, and the resulting mixed solution and the precipitated solid were the products. Dichloromethane was added to dissolve, and mesitylene was added as an internal standard. The yield of EG and DMT was determined by GC in the dissolved solution. The reaction results are shown in Table 3.

[0047] Examples 13-16

[0048] The following examples investigate the dosage of the alkaline auxiliary agent. The difference from Example 1 is that the dosage of potassium bicarbonate in the methanolysis reaction conditions is changed, corresponding to Examples 13-16 respectively.

[0049] Add 3 mmol PET powder, 3 mmol guaiacol, 0.45-0.9 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system is heated to 120°C and reacted at this temperature for 2 h. After the reaction is completed, cool to room temperature, and the resulting mixed solution and precipitated solid are the products. Add dichloromethane to dissolve, add mesitylene as an internal standard, and the yield of EG and DMT is determined by GC in the dissolved solution. The reaction results are shown in Table 4.

[0050] Examples 17-20

[0051] The following examples investigate the amount of methanol used. The difference from Example 1 is that the amount of methanol used in the methanolysis reaction conditions is changed, corresponding to Examples 17-20, respectively.

[0052] Add 3 mmol PET powder, 3 mmol guaiacol, 0.3 mmol potassium bicarbonate and 0.5-4.5 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system is heated to 120°C and reacted at this temperature for 2 h. After the reaction is completed, cool to room temperature, and the resulting mixed solution and precipitated solid are the products. Add dichloromethane to dissolve, add mesitylene as an internal standard, and the yield of EG and DMT is determined by GC in the dissolved solution. The reaction results are shown in Table 5.

[0053] Examples 21-24

[0054] The following examples investigate different acidic adjuvants. The difference from Example 1 is that guaiacol in the methanolysis reaction conditions is changed to other acidic adjuvants, which correspond to Examples 21-24 respectively.

[0055] Add 3 mmol PET powder, 3 mmol acidic additive, 0.3 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system was heated to 120°C and reacted at this temperature for 2 h. After the reaction was completed, it was cooled to room temperature, and the resulting mixed solution and precipitated solid were the products. Dichloromethane was added to dissolve, and mesitylene was added as an internal standard. The yield of EG and DMT was determined by GC in the dissolved solution. The reaction results are shown in Table 6.

[0056] Examples 25-32

[0057] The following examples investigate different alkaline catalysts. The difference from Example 1 is that potassium bicarbonate in the methanolysis reaction conditions is changed to other alkaline catalysts, corresponding to Examples 25-32 respectively.

[0058] Add 3 mmol PET powder, 3 mmol guaiacol, 0.3 mmol alkaline catalyst and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system was heated to 120°C and reacted at this temperature for 2 h. After the reaction was completed, the temperature was lowered to room temperature, and the resulting mixed solution and the precipitated solid were the products. Dichloromethane was added to dissolve, and mesitylene was added as an internal standard. The yield of EG and DMT was determined by GC in the dissolved solution. The reaction results are shown in Table 7.

[0059] Examples 33-35

[0060] The following examples investigate the coordination effects of different acidic additives and alkaline catalysts. The difference from Example 1 is that different combinations of acidic additives and alkaline catalysts are applied to the methanolysis reaction, corresponding to Examples 33-35 respectively.

[0061] Add 3 mmol PET powder, 3 mmol acidic additive, 0.3 mmol alkaline catalyst and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. The reaction system was heated to 120°C and reacted at this temperature for 2 h. After the reaction was completed, it was cooled to room temperature, and the resulting mixed solution and precipitated solid were the products. Dichloromethane was added to dissolve, and mesitylene was added as an internal standard. The yield of EG and DMT was determined by GC in the dissolved solution. The reaction results are shown in Table 8.

[0062] Examples 36-40

[0063] The following examples investigate the types of polyesters. The difference from Example 1 is that the PET in the methanolysis reaction conditions is changed to other polyester types: polybutylene terephthalate (PBT), polyethylene succinate (PES), polyethylene adipate (PEA), polycarbonate (PC), polybutylene adipate / terephthalate (PBAT), corresponding to Examples 36-40, respectively.

[0064] Add 3 mmol polyester, 3 mmol guaiacol, 0.3 mmol potassium bicarbonate and 3 mL methanol into a pressure-resistant glass tube equipped with a stirrer, place it in an oil bath, and start stirring and heating. After the reaction is completed, cool to room temperature, and the resulting mixed solution and precipitated solid are the product. Add chloroform to dissolve, add mesitylene as an internal standard, and the solution is measured by nuclear magnetic resonance for the yield of dicarboxylic acid ester products. The reaction results are shown in Table 9.

[0065] Examples 41-45

[0066] The following examples investigate real plastics, and the difference from Example 1 is that the PET in the methanolysis reaction conditions is changed to a real PET plastic product, corresponding to Examples 41-45 respectively.

[0067] The discarded PET plastic products were crushed into centimeters in advance, and 3 mmol of the centimeter-level crushed materials of PET plastic products, 3 mmol of guaiacol, 0.3 mmol of potassium bicarbonate and 3 mL of methanol were added to a pressure-resistant glass tube equipped with a stirrer, placed in an oil bath, and stirred and heated. The reaction system was heated to 120°C and reacted at this temperature for 2 h. After the reaction was completed, the temperature was cooled to room temperature, and the resulting mixed solution and the precipitated solid were the products. Dichloromethane was added to dissolve, and mesitylene was added as an internal standard. The yield of EG and DMT was determined by GC in the dissolved solution, and the results are shown in Table 10.

[0068] Embodiment 46

[0069] 5.3 mmol PET transparent plastic bottle flakes and colored plastic bottle flakes, 5.2 mmol guaiacol, 0.52 mmol potassium bicarbonate and 5.2 L methanol were added to an autoclave reactor equipped with an electromagnetic stirrer, a thermocouple and a program temperature controller. After the autoclave reactor was placed, stirring and heating were turned on. The reaction system was heated to 120 ° C and reacted at this temperature for 4 h. After the reaction was completed, the temperature was cooled to room temperature, and the obtained mixed solution and the precipitated solid were the products. The DMT product was obtained by suction filtration, washing and recrystallization, and the yield was calculated by weighing method. The results show that the DMT yield obtained from the transparent plastic bottle flakes of this embodiment is 93%, and the DMT yield obtained from the colored plastic bottle flakes is 91%.

[0070] There are significant differences in the recycling process between transparent plastic and colored plastic bottle flakes, which is mainly determined by their raw material composition, added colorants and possible impurities. Colored plastic bottle flakes are often more difficult to handle due to their complex composition. Specifically, colorants may interfere with the depolymerization reaction, reduce the activity of the catalyst, or even trigger undesirable side reactions, thereby affecting the depolymerization efficiency and the purity of the product. At the same time, colored plastics often carry more impurities such as labels, adhesives and oil stains when recycled, which require additional processing steps.

[0071] The experimental results show that the method of the present invention is not only applicable to transparent plastics, but also shows good depolymerization effects on a variety of polyester wastes including colored bottle flakes. Even when faced with high-crystallinity materials, such as PET woven tapes, the method of the present invention can achieve high yields. Therefore, the method of the present invention provides a powerful tool for processing complex polyester wastes, especially showing significant advantages in processing colored plastic bottle flakes, effectively improving recycling efficiency and product quality.

[0072] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A method for recovering waste polyester by methanolysis by acid-base synergistic catalysis, characterized in that: The following steps are involved: Polyester waste plastics, an acidic auxiliary agent and an alkaline catalyst are added to methanol to carry out a depolymerization reaction to obtain dicarboxylic acid esters, wherein the acidic auxiliary agent is a phenolic substance and the alkaline catalyst is a strong base, acetate, phosphate, carbonate, hypochlorite, aluminate, alcohol salt or phenol salt.

2. The method according to claim 1, characterized in that The polyester waste plastic is made of polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyethylene succinate or polyethylene adipate.

3. The method according to claim 1, characterized in that The phenolic substances include at least one of guaiacol, methyl guaiacol, ethyl guaiacol, hydroquinone, pyrogallol, tannic acid, pomegranate polyphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, p-bromophenol, p-cresol, phenol, 2-ethylphenol, 4-aminophenol, dichlorophenol, trichlorophenol, pentachlorophenol, p-methoxyphenol or bisphenol A.

4. The method according to claim 1, characterized in that The strong base includes at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide or calcium hydroxide; and / or, the acetate comprises at least one of lithium acetate, sodium acetate, potassium acetate, cesium acetate, calcium acetate or zinc acetate; and / or, the phosphate includes at least one of lithium phosphate, sodium phosphate, potassium phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate or cesium phosphate; and / or, the carbonate comprises at least one of lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, cesium bicarbonate, lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate or magnesium carbonate; And / or, the hypochlorite comprises at least one of sodium hypochlorite or potassium hypochlorite; And / or, the aluminate comprises at least one of sodium aluminate or potassium aluminate; and / or, the alkoxide comprises at least one of lithium methoxide, lithium ethoxide, lithium isopropoxide, sodium methoxide, sodium ethoxide, sodium tert-butoxide, sodium propoxide, sodium isopropoxide, potassium methoxide, potassium ethoxide, potassium tert-butoxide, potassium propoxide or potassium isopropoxide; And / or, the phenolate includes at least one of sodium catechol, sodium hydroquinone, sodium resorcinol, sodium cresol, potassium phenolate or sodium phenolate.

5. The method according to claim 1, characterized in that The molar ratio of the acidic auxiliary agent, the alkaline catalyst and the polyester waste plastic is (0.01-4): (0.01-1):1; the amount of methanol added per mmol of the polyester waste plastic is 0.1-6 mL.

6. The method according to claim 5, characterized in that The molar ratio of the acidic auxiliary agent, the alkaline catalyst and the polyester waste plastic is (0.05-1.5): (0.05-0.3): 1, and the amount of methanol added per mmol of the polyester waste plastic is 0.3-1.5 mL.

7. The method according to claim 1, characterized in that The reaction temperature of the depolymerization reaction is 60-200° C., and the reaction time is 0.5-18 h.

8. The method according to any one of claims 1 to 7, characterized in that The material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is guaiacol, and the alkaline catalyst is potassium bicarbonate or cesium bicarbonate.

9. The method according to any one of claims 1 to 7, characterized in that: The material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is methyl guaiacol, and the alkaline catalyst is potassium methoxide or potassium phenoxide.

10. The method according to any one of claims 1 to 7, characterized in that The material of the polyester waste plastic is polyethylene terephthalate, the acidic auxiliary agent is ethyl guaiacol, and the alkaline catalyst is sodium hypochlorite.

Citation Information

Patent Citations

  • Method for catalytic degradation of polyester (PET) waste textiles by carbonate under mild conditions

    CN105175268A

  • Waste polyester degradation method

    CN109134244A

  • Method for catalyzing waste PET polyester methanol alcoholysis by deep eutectic solvent

    CN110938231A

  • Method for catalyzing methanol alcoholysis of waste PET polyester by polyion liquid

    CN113735705A

  • Method for catalyzing and recycling waste polyester material by acetate ionic liquid

    CN116675603A

Cited By

  • Method for catalyzing polyester depolymerization by alkoxide

    CN121377995A

  • Method for catalyzing polyester depolymerization by halogen salt substances

    CN121377996A

  • Catalyst for catalyzing methanol hydrolysis of polyethylene glycol terephthalate as well as preparation method and application of catalyst

    CN121715212A