Sulfonic acid nonionic generators based on polysubstituted anthracene-1, 9-dicarboximide derivatives
By developing sulfonic acid nonionic acid generators based on anthracene-1,9-dicarboximide derivatives, the absorption wavelength and synthesis of existing sulfonium salt photoacid generators in high-resolution photolithography is solved. Complex problems have achieved efficient, thermally stable acid generators suitable for a variety of lithography technologies, simplifying the synthesis process.
Patent Information
- Application Number
- CN202310638792.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The existing sulfonium salt-based ionic photoacid generators have short absorption wavelengths in i-line and g-line photolithography, and are complex in thermal stability and synthesis methods, making it difficult to meet the needs of high-resolution photoresist.
A sulfonic acid nonionic acid generator based on anthracene-1,9-dicarboximide derivative has been developed, with a long absorption wavelength and is suitable for 365nm, 248nm, 193nm and extreme ultraviolet and electron beam lithography. Specific compound structures and synthetic routes improve their solubility and thermal stability.
It provides an efficient, thermally stable acid generator, suitable for a variety of lithography technologies, has good solubility and film forming properties, simplifies the synthesis process, and is suitable for industrial production.
Smart Images

Figure CN119059969A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a series of sulfonic acid non-ionic acid generators based on polysubstituted anthracene-1,9-dicarboximide derivatives. Background Art
[0002] Photoresist, also known as photoresist, is a type of etch-resistant thin film material whose solubility changes after being irradiated by energy such as light beams, electron beams, ion beams or x-rays. It is widely used in the micro-machining of integrated circuits and discrete semiconductor devices. With the rapid development of the semiconductor industry, the resolution required by photolithography technology is getting higher and higher, and the edge roughness requirements are getting smaller and smaller, which puts higher requirements on the comprehensive performance that photoresist materials can achieve.
[0003] Since the early 1960s, photoresists have also experienced a rapid development process, from negative photoresist formulations based on polyvinyl cinnamate with photosensitizers to later i-line (365nm) positive photoresist formulations of diazo naphthoquinone-phenolic resin (DNQNovolac). Starting from the 0.25μm node in the mid-1990s, the demand for higher resolution has promoted the application of chemically amplified photoresists (CAR), which have been used in more advanced technology nodes such as 7nm and even 5nm and 3nm.
[0004] Since IBM proposed the concept of "chemical amplification" in 1982, photoacid generator (PAG) (also called acid generator) has become a key component of photoresist. The so-called "chemical amplification" means that PAG decomposes to produce acid after light exposure, and the acid triggers a series of chemical reactions, causing the solubility of the photoresist material in the illuminated area and the non-illuminated area to change significantly. Then, the pattern transfer can be achieved through development. Therefore, the acid generation efficiency of the photoacid generator and the distribution of the photoacid generator in the material play an important role in the pattern quality.
[0005] Chemically amplified photoresists have higher exposure sensitivity. On the one hand, they can reduce the dependence on the output energy of short-wavelength light sources such as krypton fluoride (KrF) and argon fluoride (ArF) that are difficult to obtain. On the other hand, they can more precisely adjust the imaging quality by controlling the temperature and time of post-exposure bake (PEB), such as contrast, depth of focus, and verticality of the sidewall profile, making the photochemical reaction more precisely controllable.
[0006] At present, there are many patent reports on sulfonium salt-based ionic photoacid generators. Sulfonium salt acid generators have advantages such as good thermal stability and high acid generation efficiency. However, most sulfonium salt photoacid generators, such as triphenylsulfonium salt, have short absorption wavelengths and cannot be used in i-line and g-line lithography, and the synthesis method is relatively complicated. Summary of the invention
[0007] To solve the above problems, the present invention provides a sulfonic acid nonionic acid generator based on anthracene-1,9-dicarboximide derivatives, which has a long absorption wavelength and can be used as an acid generator in 365, 248, 193nm, extreme ultraviolet and electron beam lithography.
[0008] The technical solution of the present invention is as follows:
[0009] A compound shown in the following formula I:
[0010]
[0011] in:
[0012] R1, R3, R4 are the same or different and are independently selected from H, C 1-12 Alkyl, C 2-12 Alkenyl or C 2-12 Alkynyl;
[0013] m is 1, 2, 3 or 4; n is 1, 2 or 3;
[0014] R2 is selected from the following groups: C 1-12 Alkyl, C 3-12 Cycloalkyl, C 6-14 Aryl, C 1-12 Haloalkyl, -C 1-12 Alkyl-C 6-14 Aryl, -C 1-12 Alkyl-C 3-12 Cycloalkyl;
[0015] Rs is selected from halogen, C 1-12 Alkyl, C 1-12 Halogenated alkyl.
[0016] In one embodiment, R1 is selected from H or C 1-12 alkyl;
[0017] In a preferred embodiment, R1 is selected from hydrogen, methyl, ethyl, propyl, isopropyl, 1-butyl, 2-butyl, isobutyl, tert-butyl, 1-pentyl, isopentyl, tert-pentyl, 1-hexyl, 2-hexyl, 3-hexyl, heptyl, 2-heptyl, 3-heptyl, isoheptyl, tert-heptyl, 1-octyl, isooctyl, tert-octyl, 2-ethylhexyl, 1-nonyl, isononyl, 1-decyl or n-dodecyl.
[0018] In a preferred embodiment, R2 is selected from methyl, butyl, chloromethyl, trifluoromethyl, perfluoro-substituted butyl, p-methylphenyl, 2,4,6-triisopropylphenyl Benzyl, p-trifluoromethylphenyl, 3,5-ditrifluoromethylphenyl, Perfluorosubstituted phenyl, pentafluoroethyl, 2-chloroethyl, 2-bromoethyl, heptafluoropropyl, 3-bromopropyl, tridecafluorohexyl, heptadecafluorooctyl, 2,2,2-trifluoroethyl, 1,1-difluoroethyl, 1,1-difluoropropyl, 1,1,2,2-tetrafluoropropyl, 3,3,3-trifluoropropyl, 2,2,3,3,3-pentafluoropropyl, norbornyltetrafluoroethyl, adamantane-1,1,2,2-tetrafluoropropyl, bicyclo[2.2.1]heptane-tetrafluoromethyl.
[0019] In one embodiment, R3 and R4 are H or methyl. As an example, the compound represented by formula I is selected from the following compounds:
[0020]
[0021] The present invention also provides a method for preparing the compound represented by formula I, comprising the following steps:
[0022]
[0023] Compound II reacts with R2SO2Cl to obtain compound I;
[0024] wherein R1, R2, R3, R4, m and n are as defined above.
[0025] According to an embodiment of the present invention, the compound II is prepared by the following method:
[0026]
[0027] wherein R1, R3, R4, m and n are as defined above;
[0028] The compound of formula III is reacted with hydroxylamine hydrochloride to prepare the compound of formula II.
[0029] According to an embodiment of the present invention, the compound III is prepared by the following method:
[0030]
[0031] wherein R1, R3, R4, m and n are as defined above;
[0032] The compound of formula IV is reacted with an oxidant (such as potassium persulfate complex salt (Oxone)) to prepare compound III.
[0033] According to an embodiment of the present invention, the compound IV is prepared by the following method:
[0034]
[0035] wherein R1, R3, R4, m and n are as defined above;
[0036] The compound of formula V is reacted with C2ClO2 and CS2 to prepare compound IV.
[0037] According to an embodiment of the present invention, the compound V is prepared by the following method:
[0038]
[0039] wherein R1, R3, R4, m and n are as defined above;
[0040] Compound VI is reacted with alkyl lithium R1-Li to obtain compound V. The reaction can be carried out in the presence of a catalyst, such as Pd(PtBu3)2.
[0041] The present invention also provides use of the compound I as described above in photoresist.
[0042] In some embodiments, Compound I described herein is used as an acid generator.
[0043] The present invention also provides a photoresist composition, which comprises a photoresist main material and compound I.
[0044] The photoresist composition may include one, two or more photoresist host materials. The photoresist host material may be any photoresist host material known in the prior art.
[0045] In some embodiments, the photoresist main material is a single molecule resin (molecular glass); for example, the compound reported in ZL201380000139.X that can be used as a photoresist main material.
[0046] In one embodiment, the ratio of the acid generator (compound I) to the host material can be adjusted as needed, and the preferred mass ratio is 1:10-1:20.
[0047] In one embodiment, the photoresist composition further includes a solvent.
[0048] In some embodiments, the solvent is selected from one, two or more of the following substances: ethyl lactate, butyl acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol dimethyl ether, ethylene glycol monomethyl ether, cyclohexanone, methyl n-amyl ketone, and methyl isoamyl ketone.
[0049] The present invention also provides a photoresist film, which comprises the compound represented by formula I of the present invention or the photoresist composition as described above.
[0050] In one embodiment, the photoresist film of the present invention is composed of the compound represented by formula I of the present invention and any host material.
[0051] The invention also provides a method for preparing a photoresist film, which comprises spin coating the photoresist composition on a substrate to form a film.
[0052] In one embodiment, the substrate may be a silicon wafer or the like.
[0053] The present invention also provides the use of the above-mentioned photoresist composition and photoresist film in photolithography.
[0054] In one embodiment, the photolithography is 365nm, 254nm, and electron beam lithography. In particular, the photoresist composition and the photoresist film are used in 365nm photolithography and electron beam lithography.
[0055] The beneficial effects of the present invention are as follows:
[0056] The present invention provides a series of novel nonionic acid generators based on substituted anthracenes, namely compounds shown in formula I, which can be used as acid generators for photoresists and mixed with photoresist main materials, for example, with known single-molecule resins (molecular glasses). The compounds of the present invention can be used as acid generators for i-line lithography (i-line) and DUV lithography, and can also be used as acid generators for electron beam lithography and extreme ultraviolet lithography.
[0057] The compound of the present invention has good solubility in various polar solvents (such as PGMEA, PGME, cyclopentanone, etc.), and can be used to prepare good thin films by spin coating. The polyphenyl ring skeleton structure in the compound can effectively inhibit molecular crystallization and is easy to form a film. At the same time, the compound has a very high glass transition temperature (greater than 100° C.), so it has high thermal stability and is suitable for the requirements of photolithography processing technology.
[0058] The compound of the present invention has a simple synthesis process, and the reaction intermediates and the final product can be separated from the product and the system by recrystallization or precipitation, and is suitable for industrial production.
[0059] Terms and Definitions
[0060] Unless otherwise defined, all technical and scientific terms herein have the same meaning as commonly understood by one of ordinary skill in the art to which the claimed subject matter belongs.
[0061] "More" means three or more.
[0062] The term "halogen" includes F, Cl, Br or I.
[0063] The term "C 1-12 The term “alkyl” is understood to mean a linear or branched, saturated, monovalent hydrocarbon radical having 1 to 12 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl, etc. or their isomers. In particular, the radical has 1, 2, 3, 4, 5, 6 carbon atoms (“C 1-6 alkyl), for example methyl, ethyl, propyl, butyl, isopropyl, isobutyl, sec-butyl, tert-butyl, more particularly, the radical having 1, 2 or 3 carbon atoms (“C 1-3 alkyl"), for example methyl, ethyl, n-propyl or isopropyl.
[0064] The term "C 2-12 "Alkenyl" is understood to mean a linear or branched monovalent hydrocarbon radical which contains one or more double bonds and has 2 to 12 carbon atoms, preferably one or more double bonds and has 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, in particular 2 or 3 carbon atoms ("C 2-3"alkenyl"), it being understood that, in the case where the alkenyl contains more than one double bond, the double bonds may be separated from one another or conjugated. The alkenyl is, for example, vinyl, allyl, (E)-2-methylvinyl, (Z)-2-methylvinyl, (E)-but-2-enyl, (Z)-but-2-enyl, (E)-but-1-enyl, (Z)-but-1-enyl, pent-4-enyl, (E)-pent-3-enyl, (Z)-pent-3-enyl, -enyl, (E)-pent-2-enyl, (Z)-pent-2-enyl, (E)-pent-1-enyl, (Z)-pent-1-enyl, hex-5-enyl, (E)-hex-4-enyl, (Z)-hex-4-enyl, (E)-hex-3-enyl, (Z)-hex-3-enyl, (E)-hex-2-enyl, (Z)-hex-2-enyl, (E)-hex-1-enyl, (Z)-hex-1-enyl, isopropenyl, 2-hexenyl, (E)-pent-2-enyl, (Z)-pent-2-enyl, (E)-pent-1-enyl, (Z)-pent ...1-enyl, (Z)-pent-1-enyl, isopropenyl, 2-hexenyl, (E)-pent-2- -methylprop-2-enyl, 1-methylprop-2-enyl, 2-methylprop-1-enyl, (E)-1-methylprop-1-enyl, (Z)-1-methylprop-1-enyl, 3-methylbut-3-enyl, 2-methylbut-3-enyl, 1-methylbut-3-enyl, 3-methylbut-2-enyl, (E)-2-methylbut-2-enyl, (Z)-2-methylbut-2-enyl, (E)-1-methylbut-2-enyl 1-ethylprop-1-enyl, 1-propylvinyl, and 1-isopropylvinyl.
[0065] The term "C 2-12“Alkynyl” is understood as meaning a straight-chain or branched, monovalent hydrocarbon radical which contains one or more triple bonds and has 2 to 12 carbon atoms, for example 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, in particular 2 or 3 carbon atoms (“C2-C3-alkynyl”). Such alkynyl radicals are, for example, ethynyl, prop-1-ynyl, prop-2-ynyl, but-1-ynyl, but-2-ynyl, but-3-ynyl, pent-1-ynyl, pent-2-ynyl, pent-3-ynyl, pent-4-ynyl, hex-1-ynyl, hex-2-ynyl, hex-3-ynyl, hex-4-ynyl, hex-5-ynyl, 1-methylprop-2-ynyl, 2-methylbut-3-ynyl, 1-methylbut-3-ynyl, 1-methylbut-2-ynyl, 3-methylbut-1-ynyl, In some embodiments, the alkynyl group is ethynyl, prop-1-ynyl, prop-2-ynyl, 1-ethylprop-2-ynyl, 3-methylpent-4-ynyl, 2-methylpent-4-ynyl, 1-methylpent-4-ynyl, 2-methylpent-3-ynyl, 1-methylpent-3-ynyl, 4-methylpent-2-ynyl, 1-methylpent-2-ynyl, 4-methylpent-1-ynyl, 3-methylpent-1-ynyl, 2-ethylbut-3-ynyl, 1-ethylbut-3-ynyl, 1-ethylbut-2-ynyl, 1-propylprop-2-ynyl, 1-isopropylprop-2-ynyl, 2,2-dimethylbut-3-ynyl, 1,1-dimethylbut-3-ynyl, 1,1-dimethylbut-2-ynyl or 3,3-dimethylbut-1-ynyl. In particular, the alkynyl group is ethynyl, prop-1-ynyl or prop-2-ynyl.
[0066] The term "C 3-12 "Cycloalkyl" should be understood to mean a saturated monovalent monocyclic, bicyclic hydrocarbon ring or polycyclic hydrocarbon ring (also called condensed hydrocarbon ring) having 3-10 carbon atoms. Bicyclic or polycyclic cycloalkyl groups include paracyclic cycloalkyl, bridged cycloalkyl and spirocyclic cycloalkyl; the paracyclic refers to a condensed ring structure formed by two or more cyclic structures sharing two adjacent ring atoms (i.e., sharing one bond). The bridged ring refers to a condensed ring structure formed by two or more cyclic structures sharing two non-adjacent ring atoms. The spirocyclic refers to a condensed ring structure formed by two or more cyclic structures sharing one ring atom. For example, the C 3-20 The cycloalkyl group may be C 3-8 Monocyclic cycloalkyl, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, or C 7-12 Cycloalkyl, such as decahydronaphthalene; it can also be C 7-12 Bridged ring cycloalkyl, such as norbornane, adamantane, bicyclo[2,2,2]octane.
[0067] The term "C 6-14The term "aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 or a ring having 9 carbon atoms ("C9 aryl"), for example indanyl or indenyl, or a ring having 10 carbon atoms ("C 10 aryl), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms ("C 13 aryl), such as fluorenyl, or a ring having 14 carbon atoms ("C 14 aryl”), such as anthracenyl. When the C 6-20 When the aryl group is substituted, it may be monosubstituted or polysubstituted. Also, there is no limitation on the substitution position, for example, it may be substituted at the ortho position, para position or meta position.
[0068] The term "C 1-12 "Haloalkyl" is to be understood as "C 1-12 The case where at least one H on the "alkyl" is substituted by a halogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 is the UV absorption spectrum of compound 1.
[0070] Figure 2 Atomic force scanning probe microscopy (AFM) plan view of the film of compound 1.
[0071] Figure 3 This is an atomic force scanning probe microscope (AFM) stereogram of the film of compound 1.
[0072] Figure 4 This is a scanning electron microscope (SEM) image of 365nm (i-line) photolithography stripes of compound 1 as an acid generator forming a photoresist with other host materials.
[0073] Figure 5 This is a scanning electron microscope (SEM) image of 248nm photolithography stripes of compound 1 as an acid generator forming a photoresist with other host materials.
[0074] Figure 6 This is a scanning electron microscope (SEM) image of 365nm (i-line) photolithography stripes of compound 7 as an acid generator forming a photoresist with other host materials.
[0075] Figure 7 This is a scanning electron microscope (SEM) image of 248nm photolithography stripes of compound 7 used as an acid generator to form a photoresist with other host materials.
[0076] Figure 8 This is a scanning electron microscope (SEM) image of electron beam lithography stripes of compound 1 as an acid generator forming a photoresist with other host materials.
[0077] Fig. 9 This is a scanning electron microscope (SEM) image of electron beam lithography stripes of compound 7 as an acid generator forming a photoresist with other host materials. DETAILED DESCRIPTION
[0078] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0079] Example 1 Preparation of Compound (2)
[0080] The intermediate compound 2-IV was prepared by the following synthetic route:
[0081]
[0082] To a cold (0°C) stirred solution of compound 2-V (2.34 g) and oxalyl chloride (4.8 mL) in CS2 (21 mL) was added anhydrous AlCl3 (2.13 g), followed by 2 hours of adding CS2 (21 mL) and AlCl3 (1.6 g), and stirring was continued at 0°C for 2 h, then stirred at room temperature overnight. A dilute aqueous hydrochloric acid solution (2 M) was added, and the orange precipitate formed was collected by filtration, washed with water, and then digested with 100 mL 5% NaOH. The solid was washed with water and dried in air to give intermediate compound 2-IV with a yield of 80%. 1 HNMR (CDCl3, 400MHz): δppm 9.27 (m, 1H), 8.40 (db, 2H), 7.85 (b, 1H), 7.64 (m, 1H), 7.54 (dt, 2H), 2.72 (s, 3H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z = 274.1, calculated value: (C 19 H 14 O2) m / z = 274.1 ([M] + ).
[0083] Example 2 Preparation of intermediate compound 2-III, the synthesis route is as follows:
[0084]
[0085] Potassium hydrogen persulfate (5.52 g, 4 eq) was added to a solution of compound 2-IV (2.59 g, 1 eq) in methanol (300 mL), and the mixture was refluxed at 70° C. for 72 hours. After cooling, water was added, and the suspension was collected by filtration, washed with water and dried in air to give compound 2-III with a yield of 80%. 1 HNMR (CDCl3, 400MHz): δppm 8.97 (m, 1H), 8.55 (db, 2H), 8.11 (b, 1H), 7.67 (m, 1H), 7.61 (dt, 2H), 7.64 (m, 1H), 7.54 (dt, 2H), 2.72 (s, 3H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z=305.1, calculated value: (C 19 H 14 O3) m / z = 304.1 ([M] + ).
[0086] Example 3 Preparation of intermediate compound 2-II, the synthesis route is as follows:
[0087]
[0088] Hydroxylamine hydrochloride (272 mg, 1 eq) was added to a mixture of compound 2-III (1.2 g, 1 eq) and pyridine (10 mL), and the mixture was heated at 100 ° C for 15 hours. The reaction mixture was poured into 50 mL of 1 M HCl. The precipitate was filtered and washed with water, and the crude product was purified by column chromatography (20% ethyl acetate / hexane) to obtain compound 2-II with a yield of 80%. 1 HNMR (CDCl3, 400MHz): δppm 10.5 (s, 1H) 9.27 (m, 1H), 8.40 (db, 2H), 7.85 (b, 1H), 7.64 (m, 1H), 7.54 (dt, 2H), 2.72 (s, 3H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z=305.1, calculated value: (C 19 H 15 NO3) m / z = 305.1 ([M] + ).
[0089] Example 4 Compound (2) was prepared by the following synthesis route:
[0090]
[0091] At 0 ℃, Et is added dropwise to a mixture of trifluoromethylsulfonyl chloride (0.64ml, 1.5mmol), compound 2-II (1.14g, 1eq) and dry DCM N (2.24mL, 2mmol). The mixture is then stirred at room temperature overnight. After the reaction is complete, it is quenched with cold water, diluted with DCM, the organic layer is separated, and dried over Na SO, and the solvent is removed under vacuum to obtain orange crude sulfonate. The crude product is purified by column chromatography (20% ethyl acetate / hexane) to obtain compound (2), which is an orange solid with a yield of 65%. 1 HNMR (400 MHz, DMSO-d6) δ (ppm) 9.59 (d, 1H), 9.14 (s, 1H), 8.55-8.67 (m, 2H), 8.19 (d, 1H), 7.79-7.90 (m, 2H), 7.66 (t, 1H), 2.72 (s, 3H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z = 421.1, calculated value: (C 20 H 14 F3NO4S)m / z=421.1([M] + ).
[0092] Example 5 Preparation of Compound (1)
[0093] The synthetic route is as follows:
[0094]
[0095] Compound 1-II (N-hydroxyanthracene-1,9-dicarboximide) was also prepared by referring to the preparation method of Example 1-3 above.
[0096] Under an ice bath, Et3N (0.52 mL, 2 eq) was added dropwise to a mixture of trifluoromethanesulfonyl chloride (1.5 eq), N-hydroxyanthracene-1,9-dicarboximide (250 mg, 1 eq) and 5 mL of dry dichloromethane. The mixture was then stirred at room temperature overnight. After the reaction was completed, it was quenched with 20 mL of cold water, diluted with 20 mL of dichloromethane, extracted three times to separate the organic layer, and dried over anhydrous Na2SO4, and the solvent was removed by rotary evaporation to obtain an orange crude product. The crude product was purified by column chromatography (V 二氯甲烷:石油醚 =1:3), the product was obtained as an orange solid with a yield of 60%. 1 HNMR (DMSO-d6 400MHz) δ (ppm) 9.59 (d, 1H), 9.14 (s, 1H), 8.55-8.67 (m, 2H), 8.19 (d, 1H), 7.79-7.90 (m, 2H), 7.66 (t, 1H), MS (MALDI-TOF): m / z = 395.0, calculated value: C17 H8F3NO5S m / z=395.0([M] + ).
[0097] Example 6 Preparation of Compound (3)
[0098] The synthetic route is as follows:
[0099]
[0100] Under ice bath, Et3N (0.52mL, 2eq) was added dropwise to a mixture of monochloromethanesulfonyl chloride (3518-65-8) (1.5eq), 2-II (250mg, 1eq) and 5mL dry dichloromethane. The mixture was then stirred at room temperature overnight. After the reaction was complete, it was quenched with 20mL cold water, diluted with 20mL dichloromethane, extracted three times to separate the organic layer, and dried over anhydrous Na2SO4, and the solvent was removed by rotary evaporation to obtain an orange crude product. The crude product was purified by column chromatography (V 二氯甲烷:石油醚 =1:3), the product was obtained as an orange solid with a yield of 60%. 1 HNMR (DMSO-d6 400MHz) δ (ppm) 9.59 (d, 1H), 9.14 (s, 1H), 8.55-8.67 (m, 2H), 8.19 (d, 1H), 7.79-7.90 (m, 2H), 7.66 (t, 1H), 5.14 (s, 2H), 2.72 (s, 3H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z = 417.0, calculated value: C 20 H 16 ClNO5S m / z=417.0([M] + ).
[0101] Example 7 Preparation of Compound (7)
[0102] The synthetic route is as follows:
[0103]
[0104] Compound 7-II was also prepared by referring to the preparation method of Example 1-3 above.
[0105] Under ice bath, Et3N (0.52mL, 2eq) was added dropwise to a mixture of perfluorobutylsulfonyl chloride (1.5eq), 7-II (220mg, 1eq) and 5mL dry dichloromethane. The mixture was then stirred at room temperature overnight. After the reaction was complete, it was quenched with 20mL cold water, diluted with 20mL dichloromethane, extracted three times to separate the organic layer, and dried over anhydrous Na2SO4, and the solvent was removed by rotary evaporation to obtain an orange crude product. The crude product was purified by column chromatography (V二氯甲烷:石油醚 =1:3), the product was obtained as an orange solid with a yield of 65%. 1 HNMR (DMSO-d6 400MHz) δ (ppm) 9.23 (d, 1H), 9.02 (s, 1H), 8.55-8.67 (m, 2H), 8.19 (d, 1H), 7.79-7.90 (m, 2H), 7.66 (t, 1H), 3.14 (m, 2H), 2.51 (s, 12H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z = 629.5, calculated value: C 26 H 20 F9NO5S m / z=629.5([M] + ).
[0106] Example 8 Preparation of Compound (8)
[0107] The synthetic route is as follows:
[0108]
[0109] Compound 8-II was also prepared by referring to the preparation method of Example 1-3 above.
[0110] Under ice bath, Et3N (0.52mL, 2eq) was added dropwise to a mixture of methylsulfonyl chloride (1.5eq), 8-II (240mg, 1eq) and 5mL dry dichloromethane. The mixture was then stirred at room temperature overnight. After the reaction was complete, it was quenched with 20mL cold water, diluted with 20mL dichloromethane, extracted three times to separate the organic layer, and dried over anhydrous Na2SO4, and the solvent was removed by rotary evaporation to obtain an orange crude product. The crude product was purified by column chromatography (V 二氯甲烷:石油醚 =1:3), the product was obtained as an orange solid with a yield of 65%. 1 HNMR (DMSO-d6 400MHz) δ (ppm) 9.23 (d, 1H), 9.02 (s, 1H), 8.55-8.67 (m, 2H), 8.19 (d, 1H), 7.79-7.90 (m, 2H), 7.66 (t, 1H), 3.51 (s, 3H), 3.14 (m, 2H), 2.51 (s, 18H), 2.66 (s, 3H), 2.62 (s, 3H). MS (MALDI-TOF): m / z = 629.5, calculated value: C 26 H 20 F9NO5S m / z=629.5([M] + ).
[0111] Example 9
[0112] The ultraviolet absorption diagram of the acid generator (Compound 1) prepared in Example 5 in acetonitrile is shown in the attached Figure 1 The results show that it has high absorption in the i-line and is very suitable as an acid generator for i-line lithography.
[0113] Example 10
[0114] Compound 1 in Example 5 was mixed with a molecular glass main material (SP8-Boc) (SP8-Boc is a structure disclosed in the literature Molecular Glass Resists Based on 9,9'-Spirobifluorene Derivatives: Pendant Effect and Comprehensive Evaluation in Extreme Ultraviolet Lithography. ACS Appl. Polym. Mater. 2019, 1 (3), 526-534) and dissolved in propylene glycol monomethyl ether acetate (PGMEA) to obtain a main material concentration of 30 mg / ml solution (the mass of compound 1 accounts for 10% of the main material), filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, and spin coating was performed on an acid-base treated silicon substrate to form a film, and the uniformity of the film was analyzed by atomic force microscopy AFM. The plane and stereoscopic images are shown in the attached drawings. Figure 2 and 3 As can be seen from the figure, the obtained film is very uniform. This is mainly because the polyphenyl ring skeleton structure in the compound can effectively inhibit molecular crystallization, so it is easy to form a film.
[0115] Embodiment 11
[0116] i-line lithography: Compound 1 in Example 5 is used as an acid generator and mixed with 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene monomolecular resin reported in Patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA) (Compound 1 is completely dissolved in the solvent). Among them, the content of the monomolecular resin main material is 30 mg / ml, and the content of the acid generator is 2.25 mg / ml. It is filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating liquid, and a spin coating film is formed on a silicon substrate treated with acid and alkali, and baked at 100°C for 3 minutes. The prepared film is exposed on a 365nm exposure machine. The exposure cycle is 2 μm, and very uniform lithography stripes are obtained. Figure 4 The width of the photolithography stripe is about 1 μm.
[0117] Example 12
[0118] 254nm photolithography: Compound 1 in Example 5 was used as an acid generator and mixed with the 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene single-molecule resin reported in Patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA) (Compound 1 was completely dissolved in the solvent). The content of the single-molecule resin main material was 30 mg / ml, and the content of the acid generator was 2.25 mg / ml. The solution was filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, which was spin-coated on an acid-base treated silicon substrate, baked at 100°C for 3 minutes, and the prepared film was exposed to a 254nm light source. The exposure period was 2 μm, and very uniform photolithography stripes were obtained. Figure 5 The width of the photolithography stripe is about 1 μm.
[0119] Embodiment 13
[0120] i-line lithography: Compound 1 in Example 7 is used as an acid generator and mixed with 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene monomolecular resin reported in Patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA) (Compound 1 is completely dissolved in the solvent). Among them, the content of the monomolecular resin main material is 30 mg / ml, and the content of the acid generator is 2.25 mg / ml. It is filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating liquid, and a spin coating film is formed on a silicon substrate treated with acid and alkali, and baked at 100°C for 3 minutes. The prepared film is exposed on a 365nm exposure machine. The exposure cycle is 2 μm, and very uniform lithography stripes are obtained. Figure 6 The width of the photolithography stripe is about 1 μm.
[0121] Embodiment 14
[0122] 254nm photolithography: Compound 7 in Example 7 was used as an acid generator and mixed with 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene monomolecular resin reported in Patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA) (Compound 1 was completely dissolved in the solvent). The content of the monomolecular resin main material was 30 mg / ml, and the content of the acid generator was 2.25 mg / ml. The solution was filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, which was spin-coated on an acid-base treated silicon substrate, baked at 100°C for 3 minutes, and the prepared film was exposed to a 254nm light source with an exposure period of 2 μm to obtain very uniform photolithography stripes, as shown. Figure 7 The width of the photolithography stripe is about 1 μm.
[0123] Embodiment 15
[0124] Electron beam lithography: Compound 1 in Example 5 was used as an acid generator and mixed with 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene monomolecular resin reported in patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA). The content of the monomolecular resin main material was 30 mg / ml, and the content of the acid generator was 2.25 mg / ml. The photoresist solution was filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, which was spin-coated on an acid-base treated silicon substrate, baked at 100°C for 3 minutes, and the prepared film was subjected to an electron beam exposure experiment with an exposure period of 80 nm to obtain very uniform lithography stripes, as shown. Figure 8 , the width of the lithography stripe is about 32nm.
[0125] Example 16
[0126] Electron beam lithography: Compound 7 in Example 7 was used as an acid generator and mixed with 2,7,2',7'-tetra-(3,4-di-tert-butyl carbonate phenyl)-9,9'-spirofluorene monomolecular resin reported in patent ZL201380000139.X, and dissolved in propylene glycol monomethyl ether acetate (PGMEA). The content of the monomolecular resin main material was 30 mg / ml, and the content of the acid generator was 2.25 mg / ml. The photoresist solution was filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, which was spin-coated on an acid-base treated silicon substrate, baked at 100°C for 3 minutes, and the prepared film was subjected to an electron beam exposure experiment with an exposure period of 100 nm to obtain very uniform lithography stripes, as shown. Fig. 9 , the width of the lithography stripe is about 45nm.
[0127] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A compound as shown in the following formula I: in: R1, R3, R4 are the same or different and are independently selected from H, C 1-12 Alkyl, C 2-12 Alkenyl or C 2-12 Alkynyl; m is 1, 2, 3 or 4; n is 1, 2 or 3; R2 is selected from the following groups which are unsubstituted or optionally substituted by one, two or more Rs: 1-12 Alkyl, C 3-12 Cycloalkyl, C 6-14 Aryl, C 1-12 Haloalkyl, -C 1-12 Alkyl-C 6-14 Aryl, -C 1-12 Alkyl-C 3-12 Cycloalkyl; Rs is selected from halogen, C 1-12 Alkyl, C 1-12 Halogenated alkyl.
2. The compound according to claim 1, characterized in that R1 is selected from H or C 1-12 alkyl.
3. The compound according to claim 1, characterized in that R1 is selected from hydrogen, methyl, ethyl, propyl, isopropyl, 1-butyl, 2-butyl, isobutyl, tert-butyl, 1-pentyl, isopentyl, tert-pentyl, 1-hexyl, 2-hexyl, 3-hexyl, heptyl, 2-heptyl, 3-heptyl, isoheptyl, tert-heptyl, 1-octyl, isooctyl, tert-octyl, 2-ethylhexyl, 1-nonyl, isononyl, 1-decyl or n-dodecyl; R2 is selected from methyl, butyl, chloromethyl, trifluoromethyl, perfluoro-substituted butyl, p-methylphenyl, 2,4,6-triisopropylphenyl, benzyl, p-trifluoromethylphenyl, 3,5-ditrifluoromethylphenyl, perfluorosubstituted phenyl, pentafluoroethyl, 2-chloroethyl, 2-bromoethyl, heptafluoropropyl, 3-bromopropyl, tridecafluorohexyl, heptadecafluorooctyl, 2,2,2-trifluoroethyl, 1,1-difluoroethyl, 1,1-difluoropropyl, 1,1,2,2-tetrafluoropropyl, 3,3,3-trifluoropropyl, 2,2,3,3,3-pentafluoropropyl, norbornyltetrafluoroethyl, adamantane-1,1,2,2-tetrafluoropropyl, bicyclo[2.2.1]heptane-tetrafluoromethyl; R3 and R4 are H or methyl.
4. The compound according to any one of claims 1 to 3, characterized in that Selected from the following compounds:
5. A method for preparing a compound of formula I according to any one of claims 1 to 4, characterized in that: The steps include: Compound II reacts with R2SO2Cl to obtain compound I; Wherein, R1, R2, R3, R4, m and n have the meanings as described in any one of claims 1-4.
6. Use of the compound of formula I according to any one of claims 1 to 4 in photoresist; The compounds are useful as acid generators in photoresists.
7. A photoresist composition, characterized in that: Including the compound shown in formula I according to any one of claims 1 to 4.
8. The photoresist composition according to claim 7, characterized in that The photoresist composition further includes a solvent; The solvent is selected from one, two or more of the following substances: ethyl lactate, butyl acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol dimethyl ether, ethylene glycol monomethyl ether, cyclohexanone, methyl n-amyl ketone, methyl isoamyl ketone; Preferably, the photoresist composition further comprises one or more other photoresist host materials.
9. A photoresist film, characterized in that: Including the compound shown in formula I according to any one of claims 1 to 4.
10. Use of the photoresist composition according to claim 7 or 8, or the photoresist film according to claim 9 in photolithography; The lithography is 365nm, 248nm, 193nm, extreme ultraviolet and electron beam lithography.
Citation Information
Patent Citations
Multifunctional photo-acid generator and photoresist composition comprising same for thick film
CN110325910A
Sulfonium salt-based monomolecular resin acid producing agent and photoresist composition thereof
CN111978228A
Photoelectrographic elements utilizing nonionic sulfonic acid photogenerators
WO1993009474A1