Method for preparing ethylene carbonate through direct reaction of carbon dioxide and ethylene glycol

The esterification reaction of CO2 and ethylene glycol is catalyzed by cobalt-cerium bimetallic catalyst, combined with the 2-CP dehydration reaction, and the problems of expensive raw materials and harsh reaction conditions in the existing vinyl carbonate preparation methods are solved, achieving efficient and environmentally friendly carbonic acid Preparation of vinyl ester, suitable for industrial production.

CN119060011AActive Publication Date: 2024-12-03ZHEJIANG DONGJIANG GREEN PETROCHEMICAL TECHNOLOGY INNOVATION CENTER CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410943065.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-12-03
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing vinyl carbonate preparation methods have problems such as expensive raw materials, harsh reaction conditions, many by-products, complex production processes and environmental pollution, making it difficult to achieve high yield and high selectivity industrial production.

Method used

Using cobalt-cerium bimetallic catalyst, vinyl carbonate is prepared by esterification reaction of CO2 and ethylene glycol and coupled with 2-CP dehydration reaction. The nanorod structure and acid-base sites of Co-CeO2 catalyst are used to achieve efficient catalysis. .

Benefits of technology

Overcome the shortcomings of the traditional method and achieve high yield and high selectivity preparation of vinyl carbonate under mild conditions. It is suitable for industrial production and takes into account both economic and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004944779630000021
    Figure BDA0004944779630000021
  • Figure BDA0004944779630000071
    Figure BDA0004944779630000071
  • Figure BDA0004944779630000081
    Figure BDA0004944779630000081
Patent Text Reader

Abstract

The invention provides a method for preparing ethylene carbonate (EC) through direct reaction of carbon dioxide (CO2) and ethylene glycol (EG). CO2, EG, 2-cyanopyridine (2-CP) and a catalyst are mixed, CO2 and ethylene glycol are subjected to a cyclization dehydration reaction under the action of the catalyst, and an ethylene carbonate (EC) product is prepared with high selectivity and high yield; meanwhile, a hydration reaction of a dehydrating agent 2-CP is coupled, and 2-CP is hydrated to generate 2-pyridinecarboxamide (2-PA); and 2-PA is separated, and 2-CP is further prepared through a dehydration reaction for cyclic utilization. The method can avoid the problems of harsh reaction conditions, difficult product separation, expensive raw materials, environmental pollution and the like in the traditional EC production method, is an economic and environment-friendly EC production method, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical industry, in particular to a method for preparing ethylene carbonate by direct reaction of carbon dioxide and ethylene glycol, wherein the method adopts a cobalt-cerium bimetallic catalyst as a catalyst. Background Art

[0002] Ethylene carbonate (EC) is an important organic carbonate. Its excellent physical and chemical properties make it applicable in many fields. For example, EC can be used as a decarbonizing agent in natural gas, synthesis gas and other fields; as a good absorbent and solvent for organic matter; as a lithium-ion battery electrolyte in the battery industry; and as a plasticizer, spinning solvent, oily solvent, olefin and aromatic hydrocarbon extractant. EC is an environmentally friendly chemical raw material with many production processes that are constantly evolving to meet market demand.

[0003] The synthesis methods of ethylene carbonate mainly include: phosgene synthesis method, ester exchange method, halohydrin method, direct oxidation of ethylene and carbon dioxide method, ethylene oxide and carbon dioxide cycloaddition method, urea alcoholysis method, etc. Patent publication number CN113842858A discloses a reaction tower with a shallow reaction pool, which adopts urea alcoholysis method to prepare ethylene carbonate, and greatly improves the yield of ethylene carbonate by graded reaction, up to more than 95%. However, this method is costly, the by-product ammonia gas causes the catalyst to deactivate or dissolve, and the separation process is complicated. Patent publication number CN107915707A discloses a method of using a bimetallic catalyst as M 1 O.M. 2 O(where M 1 At least one selected from Ca, Mg, Sr or Ba; M 2 At least one selected from Zr or Ti), ethylene carbonate is prepared by ethylene oxide and carbon dioxide cycloaddition method, which improves the catalytic activity and can reach 96.8% ethylene oxide conversion rate and 98.7% ethylene carbonate selectivity. However, this method has harsh production operating conditions, high risk factor of raw material ethylene oxide, and many by-products. Other preparation methods have their own serious disadvantages. For example, the raw materials of the phosgene method are highly toxic, and the by-products are corrosive to the equipment; the raw materials of the ester exchange method are expensive, and the production process is more polluting to the environment; the reaction conditions of the halogenated alcohol method are harsh, and there are many by-products; the production process of the direct oxidation of ethylene and carbon dioxide is complicated, and there is also the risk of explosion.

[0004] The method of directly synthesizing ethylene carbonate from carbon dioxide and ethylene glycol takes into account both economic and environmental performance and is a promising approach. In addition, this method has been successfully practiced in the reaction of monoalcohols (such as methanol, ethanol, etc.) with carbon dioxide. Therefore, how to obtain high-yield and high-selectivity ethylene carbonate under mild conditions by changing the catalyst preparation method and exploring suitable reaction conditions is an important step in promoting the development of the carbonate industry. Summary of the invention

[0005] The present invention proposes a novel method for preparing ethylene carbonate, using cobalt-doped cerium dioxide as a catalyst to achieve CO 2 The esterification reaction with ethylene glycol is coupled with the dehydration reaction of 2-CP. This method overcomes many disadvantages of traditional production methods, such as expensive raw materials, harsh reaction conditions, difficult product separation, and environmental pollution, taking into account both economic and environmental protection, and has broad application prospects.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for synthesizing ethylene carbonate using a cobalt-cerium bimetallic catalyst, comprising:

[0008] 1) CO 2 EG, 2-cyanopyridine (2-CP) and the catalyst are mixed, and CO 2 It undergoes cyclodehydration reaction with ethylene glycol to produce ethylene carbonate (EC) product;

[0009] 2) Simultaneously, the hydration reaction of the dehydrating agent 2-CP is coupled, and 2-CP is hydrated to generate 2-pyridinecarboxamide (2-PA).

[0010] Preferably, the Co-CeO 2 The catalyst was prepared by the following method:

[0011] Cobalt (II) nitrate hexahydrate and cerium (III) nitrate hexahydrate with a molar ratio of cobalt to cerium of 0.03 to 0.1:1 are dissolved in deionized water to obtain a mixed solution, which is then added dropwise to a NaOH aqueous solution, stirred at 20 to 40°C for 20 to 40 minutes, and then transferred to a hydrothermal autoclave for aging for 10 to 15 hours. The turbid liquid is separated by centrifugation, and then washed, dried and calcined to obtain a target 3 to 10% Co-CeO 2 catalyst.

[0012] The process of washing, drying and calcining is as follows:

[0013] The product is washed with anhydrous ethanol and deionized water until neutral, freeze-dried for 20 to 30 hours, and finally calcined in air at 550 to 650° C. for 3 to 10 hours.

[0014] Preferably, the divalent cobalt salt or its hydrate is cobalt (II) nitrate hexahydrate;

[0015] The trivalent cerium salt or its hydrate is cerium (III) nitrate hexahydrate.

[0016] Prepared with 5% Co-CeO 2 The catalyst catalyzes the reaction of CO in the presence of a certain amount of solvent and a dehydrating agent, 2-cyanopyridine (2-CP). 2 The catalyst dosage is 0.1g-0.5g, the reaction pressure is 1Mpa-4Mpa, the reaction temperature is 100℃-160℃, the reaction time is 0.5h-5h, and the stirring speed is 400-800rpm.

[0017] In the scheme, the solvent is one of tetrahydrofuran (THF), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO), preferably DMF.

[0018] Preferably, the molar ratio of ethylene glycol to 2-CP is 1:1.5 to 3;

[0019] The ratio of ethylene glycol to solvent is 1-3 mmol: 1-4 mL;

[0020] The Co-CeO 2 The usage ratio of the catalyst to the ethylene glycol is 1-3 g: 50-150 mmol.

[0021] Preferably, the reaction pressure is 1Mpa-4Mpa, the reaction temperature is 100°C-160°C, and the reaction time is 0.5h-5h. More preferably, the reaction pressure is 3-4Mpa, the reaction temperature is 120-140°C, and the reaction time is 1-2h.

[0022] Preferably, the reaction is carried out at a rotation speed of 400-800 rpm.

[0023] Preferably, the method further comprises the following steps:

[0024] 2-PA is separated from the product and further dehydrated to produce 2-CP for recycling.

[0025] The reaction equation for this process is:

[0026]

[0027] Figure 3 This is the reaction mechanism of the present invention.

[0028] The advantages of adopting the method of the present invention are:

[0029] (1) The catalyst prepared by the present invention has a small size and a uniform nanorod structure, and has numerous surface oxygen vacancies and acid-base sites, which can effectively adsorb and activate ethylene glycol and CO 2 , which can effectively catalyze the reaction of ethylene glycol and CO 2 The reaction is carried out in combination with a dehydrating agent to obtain ethylene carbonate with high yield and selectivity.

[0030] (2) The present invention uses ethylene glycol and CO 2 Compared with the traditional method, the method of preparing ethylene carbonate by direct reaction overcomes the disadvantages of expensive raw materials, harsh reaction conditions, difficult product separation, environmental pollution, etc., and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0032] Figure 1 The present invention is a process flow chart for preparing ethylene carbonate.

[0033] Figure 2 The 5% Co-CeO prepared by the present invention 2 TEM images and particle size distribution of the catalysts.

[0034] Figure 3 The 5% Co-CeO prepared by the present invention 2 HAADF diagram of the catalyst.

[0035] Figure 4 The 5% Co-CeO prepared by the present invention 2 Catalyst catalyzes CO 2 Mechanism diagram for the preparation of ethylene carbonate by reaction with ethylene glycol. DETAILED DESCRIPTION

[0036] Figure 1 The process flow chart of preparing ethylene carbonate of the present invention is as follows:

[0037] CO 2 EG, catalyst, dehydrating agent and solvent are mixed, and CO 2The cyclodehydration reaction takes place with ethylene glycol. After the reaction is completed, the gas-liquid separation is performed to obtain carbon dioxide which is returned to the cyclodehydration reaction for further application. The obtained liquid substance is further separated by the separation unit to obtain the crude ethylene carbonate (EC) and the 2-PA solution. The crude ethylene carbonate (EC) is refined in the separation unit to obtain the EC product. The 2-PA solution obtained in the separation unit is recovered by solvent, and the obtained solvent is returned to the cyclodehydration reaction for further application. At the same time, the 2-PA after solvent recovery is regenerated by the dehydrating agent, and the obtained dehydrating agent is applied to the cyclodehydration reaction. The entire process realizes the application of dehydrating agent and solvent.

[0038] The catalyst and catalytic reaction of the present invention are further described below in conjunction with the examples. This example is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention includes but is not limited to the following examples.

[0039] Example 1

[0040] Cobalt (II) nitrate hexahydrate and cerium (III) nitrate hexahydrate (wherein the mass of cerium (III) nitrate hexahydrate is 4.3g) with a molar ratio of cobalt to cerium atoms of 0.05:1 were dissolved in 25ml of deionized water, and 48g of NaOH was dissolved in 175ml of deionized water. The mixed solution of cerium nitrate and cobalt nitrate was added dropwise to the NaOH solution, stirred at room temperature for 30min, and then transferred to a hydrothermal kettle for aging for 12h. The turbid liquid was separated by centrifugation, and the product was washed with anhydrous ethanol and deionized water until neutral, and freeze-dried for 24h. Finally, it was calcined in air at 600℃ for 5 hours to obtain the target 5% Co-CeO 2 The TEM image and particle size distribution of the catalyst are shown in Figure 1 , HAADF diagram is shown in Figure 2 ,Depend on Figure 1 and Figure 2 It can be seen that the obtained Co-CeO 2 The catalyst is small in size and has a uniform nanorod structure.

[0041] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMSO solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0042] Example 2

[0043] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0044] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of dioxane solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0045] Example 3

[0046] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0047] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of THF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0048] Example 4

[0049] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0050] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of NMP solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0051] Example 5

[0052] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0053] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0054] Example 6

[0055] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0056] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0057] Example 7

[0058] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0059] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 5 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. The sample was taken back for GC detection, and the results were shown in Table 1 according to the ratio of raw materials and products.

[0060] Example 8

[0061] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0062] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2The amount of ethylene glycol was 15 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0063] Example 9

[0064] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0065] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 5 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. The sample was taken back for GC detection, and the results were shown in Table 1 according to the ratio of raw materials and products.

[0066] Example 10

[0067] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0068] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 15 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0069] Embodiment 11

[0070] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0071] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 15 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0072] Example 12

[0073] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0074] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.15 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0075] Embodiment 13

[0076] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0077] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.25 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0078] Embodiment 14

[0079] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0080] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 3 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0081] Embodiment 15

[0082] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0083] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 2 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0084] Example 16

[0085] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0086] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 130 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0087] Embodiment 17

[0088] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0089] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 110 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0090] Embodiment 18

[0091] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0092] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 2 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0093] Embodiment 19

[0094] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0095] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 0.5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0096] Comparative Example 1

[0097] Cobalt (II) nitrate hexahydrate and cerium (III) nitrate hexahydrate (4.3 g) with a molar ratio of cobalt to cerium atoms of 0.03:1 were dissolved in 25 ml of deionized water, and 48 g of NaOH was dissolved in 175 ml of deionized water. The mixed solution of cerium nitrate and cobalt nitrate was added dropwise to the NaOH solution, stirred at room temperature for 30 min, and then transferred to a hydrothermal autoclave for aging for 12 h. The turbid liquid was separated by centrifugation, and the product was washed with anhydrous ethanol and deionized water until neutral, and freeze-dried for 24 h. Finally, it was calcined in air at 600 ° C for 5 hours to obtain the target 3% Co-CeO 2 catalyst.

[0098] In a 50 ml stirred tank lined with polytetrafluoroethylene, 3% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0099] Comparative Example 2

[0100] Cobalt (II) nitrate hexahydrate and cerium (III) nitrate hexahydrate (4.3 g) with a molar ratio of cobalt to cerium atoms of 0.1:1 were dissolved in 25 ml of deionized water, and 48 g of NaOH was dissolved in 175 ml of deionized water. The mixed solution of cerium nitrate and cobalt nitrate was added dropwise to the NaOH solution, stirred at room temperature for 30 min, and then transferred to a hydrothermal autoclave for aging for 12 h. The turbid liquid was separated by centrifugation, and the product was washed with anhydrous ethanol and deionized water until neutral, and freeze-dried for 24 h. Finally, it was calcined in air at 600 ° C for 5 hours to obtain the target 10% Co-CeO 2 catalyst.

[0101] In a 50 ml stirred tank lined with polytetrafluoroethylene, 10% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0102] Comparative Example 3

[0103] Aluminum (III) nitrate nonahydrate and cerium (III) nitrate hexahydrate (4.3 g) with an aluminum-cerium atomic molar ratio of 0.05:1 were dissolved in 25 ml of deionized water, and 48 g of NaOH was dissolved in 175 ml of deionized water. The mixed solution of cerium nitrate and aluminum nitrate was added dropwise to the NaOH solution, stirred at room temperature for 30 min, and then transferred to a hydrothermal autoclave for aging for 12 h. The turbid liquid was separated by centrifugation, and the product was washed with anhydrous ethanol and deionized water until neutral, and freeze-dried for 24 h. Finally, it was calcined in air at 600 ° C for 5 hours to obtain the target 5% Al-CeO 2 catalyst.

[0104] In a 50 ml stirred kettle lined with polytetrafluoroethylene, 5% Al-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0105] Comparative Example 4

[0106] Dissolve copper (II) nitrate trihydrate and cerium (III) nitrate hexahydrate (4.3 g) with a copper-cerium atomic molar ratio of 0.05:1 in 25 ml of deionized water, and dissolve 48 g of NaOH in 175 ml of deionized water. Add the mixed solution of cerium nitrate and copper nitrate dropwise to the NaOH solution, stir at room temperature for 30 min, and then transfer to a hydrothermal autoclave for aging for 12 h. Centrifuge the turbid liquid, wash the product with anhydrous ethanol and deionized water until neutral, and freeze-dry for 24 h. Finally, calcine in air at 600 ° C for 5 hours to obtain the target 5% Cu-CeO 2 catalyst.

[0107] In a 50 ml stirred kettle lined with polytetrafluoroethylene, 5% Cu-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0108] Comparative Example 5

[0109] 5% Co-CeO 2The catalyst preparation method is the same as in Example 1.

[0110] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 Propylene carbonate was prepared by reacting with 1,3-propylene glycol. The amount of 1,3-propylene glycol was 10 mmol, the amount of solvent DMF was 10 ml, the amount of 2-CP was 20 mmol, the amount of catalyst was 0.2 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0111] Comparative Example 6

[0112] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0113] In a 50 ml stirred tank lined with polytetrafluoroethylene, 5% Co-CeO 2 Catalytic CO 2 The amount of glycerol was 10 mmol, the amount of DMF solvent was 10 ml, the amount of 2-CP was 30 mmol, the amount of catalyst was 0.34 g, the reaction pressure was 4 MPa, the reaction temperature was 140 ° C, the reaction time was 5 h, and the stirring speed was 500 rpm. The reaction samples were taken for GC detection, and the results were shown in Table 1 according to the ratio of raw materials and products.

[0114] Comparative Example 7

[0115] 5% Co-CeO 2 The catalyst preparation method is the same as in Example 1.

[0116] In a 50 ml stirred tank, 5% Co-CeO 2 Catalytic CO 2 The amount of ethylene glycol was 12 g, the amount of 2-CP was 15 g, the amount of catalyst was 0.2 g, the reaction pressure was 2 MPa, the reaction temperature was 130 ° C, the reaction time was 6 h, and the stirring speed was 500 rpm. Samples were taken for GC detection, and the reaction results were shown in Table 1 according to the ratio of raw materials and products.

[0117] Table 1 Reaction results of Examples 1 to 19 and Comparative Examples 1 to 7

[0118]

[0119]

[0120] From the results in Table 1, it can be seen that with 5% Co-CeO2 As a catalyst, 2-CP is a dehydrating agent. Under the solvation effect of DMF, ethylene glycol and carbon dioxide are catalyzed to directly synthesize EC, and a high yield of EC can be obtained while producing very few by-products. In addition, this scheme is also applicable to the reaction of other polyols and carbon dioxide. It is shown that the present invention is a scheme for efficiently synthesizing cyclic carbonates and is expected to be promoted to industrial applications.

Claims

1. A method for preparing ethylene carbonate by direct reaction of carbon dioxide and ethylene glycol, Features: include: 1) CO 2 EG, 2-cyanopyridine (2-CP) and the catalyst are mixed, and CO 2 It undergoes cyclodehydration reaction with ethylene glycol to produce ethylene carbonate (EC) product; 2) Simultaneously, the hydration reaction of the dehydrating agent 2-CP is coupled, and 2-CP is hydrated to generate 2-pyridinecarboxamide (2-PA).

2. The method according to claim 1, It is characterized in that The catalyst is Co-CeO 2 The catalyst is prepared by the following method: A divalent cobalt salt or its hydrate and a trivalent cerium salt or its hydrate with a cobalt-cerium atomic molar ratio of 0.03 to 0.1:1 are dissolved in deionized water to obtain a mixed solution, and the mixed solution is added dropwise to a NaOH aqueous solution, stirred at 20 to 40°C for 20 to 40 minutes, and then transferred to a hydrothermal kettle for aging for 10 to 15 hours, and the turbid liquid is separated by centrifugation, and then washed, dried and calcined to obtain a target 3 to 10% Co-CeO 2 catalyst.

3. The method according to claim 2, It is characterized in that The process of washing, drying and calcining is as follows: The product is washed with anhydrous ethanol and deionized water until neutral, freeze-dried for 20 to 30 hours, and finally calcined in air at 550 to 650° C. for 3 to 10 hours.

4. The method according to claim 2, It is characterized in that The divalent cobalt salt or its hydrate is cobalt (II) nitrate hexahydrate; The trivalent cerium salt or its hydrate is cerium (III) nitrate hexahydrate.

5. The method according to claim 1 or 2, It is characterized in that The reaction is carried out in a solvent, which is one of tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide.

6. The method according to claim 5, It is characterized in that The molar ratio of ethylene glycol to 2-cyanopyridine is 1:1.5-3; The usage ratio of ethylene glycol to solvent is 1-3 mmol:1-4 mL; The Co-CeO 2 The usage ratio of the catalyst to the ethylene glycol is 1-3 g: 50-150 mmol.

7. The method according to claim 1 or 2, It is characterized in that The reaction pressure is 1Mpa to 4Mpa, the reaction temperature is 100°C to 160°C, and the reaction time is 0.5h to 5h.

8. The method according to claim 7, It is characterized in that The reaction pressure is 3-4 MPa, the reaction temperature is 120-140°C, and the reaction time is 1-2 h.

9. The method according to claim 1 or 2, It is characterized in that The reaction was carried out at a rotation speed of 400-800 rpm.

10. The method according to claim 1 or 2, It is characterized in that The following steps are also included: 2-PA is separated from the product and further dehydrated to produce 2-CP for recycling.

Citation Information

Patent Citations

  • Method for synthesizing ethylene carbonate

    CN107915707A

  • Reaction tower with reaction shallow pools and method for preparing ethylene carbonate by using reaction tower

    CN113842858A

  • Catalyst and method for preparing glycerol carbonate from glycerol and carbon dioxide

    CN107715857A

  • Method for producing carbonic ester

    CN111601785A

  • Method for catalytic synthesis of dimethyl carbonate by using ultrafine cobalt-cerium bimetallic nano-catalyst

    CN111905752A