Intrinsic flame-retardant polypropylene foam material and preparation method thereof

Through multiple grafting reactions of solid phase grafting and twin screw extruder, combined with high-temperature water vapor rigidity reaction, supercritical foaming technology is used to solve the shortcomings of polypropylene materials in flame retardant modification and melt strength. , realizes the preparation of high-performance intrinsic flame-retardant polypropylene foaming material, with excellent physical and mechanical properties and environmentally friendly preparation technology.

CN119060398AActive Publication Date: 2024-12-03ZHEJIANG XINHENGTAI ADVANCED MATERIAL
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411553799.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
2044-11-04

AI Technical Summary

Technical Problem

The existing polypropylene foamed materials have shortcomings in flame retardant modification and high melt strength, especially the use of flame retardant has problems such as precipitation risks and degradation of material properties, and traditional methods are difficult to meet both flame retardant efficiency and physical machinery. Performance improvement.

Method used

Multiple grafting reactions were carried out through solid-phase grafting method and twin-screw extruder, combined with high-temperature water vapor rigid-increasing reaction, to generate halogen-free flame retardant containing nitrogen and phosphorus, and the intrinsic features were prepared using supercritical foaming technology. Flame-retardant polypropylene foaming material.

Benefits of technology

It realizes efficient flame retardant modification and material melt strength improvement, avoids the risks of material degradation and precipitation, and provides high-performance flame retardant polypropylene foaming materials, with excellent physical and mechanical properties and environmentally friendly preparation technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses an intrinsic flame-retardant polypropylene foam material and a preparation method thereof, and the preparation method comprises the following steps: uniformly mixing polypropylene powder, a peroxide initiator and a polymeric monomer A, and obtaining a grafted polymer 1 through a solid-phase grafting method; mixing the graft 1 polymer and ungrafted polypropylene powder, extruding the mixture through a twin-screw extruder, and adding a phosphoramidate flame retardant at the middle section position of the extruder through a side feeding system for grafting to obtain a graft 2 polymer; carrying out stiffening reaction on the grafted polymer 2 and excessive isocyanate groups through high-temperature water vapor; and carrying out supercritical foaming on the obtained material to obtain the foaming material. The melt strength of the material is improved through two-time grafting and a stiffening reaction, the whole preparation process has the advantages of being clean and environmentally friendly through supercritical fluid foaming, the prepared foaming material contains nitrogen and phosphorus, tests show that the halogen-free flame retardant efficiency is high, and the problems that polypropylene is low in melt strength and low in flame retardant efficiency are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high molecular polymers, in particular to an intrinsic flame retardant polypropylene foam material and a preparation method thereof. Background Art

[0002] Polypropylene is abbreviated as PP. As one of the four general-purpose plastics, it has the advantages of low VOC, light weight, excellent mechanical properties, and stable chemical properties. After foaming, the material still has good thermal stability and high mechanical properties on the basis of lightweight. The common foaming method of PP is supercritical foaming. Supercritical foaming requires PP to have a high melt strength. As a linear polymer, the melt strength of PP decreases linearly with the increase of temperature. Therefore, when foaming PP-based materials, they need to be modified with high melt strength first.

[0003] Foamed PP is currently widely used in new energy batteries, home furnishings, cushioning materials and other fields. In these application fields, PP is required to have good flame retardant properties. Due to the long carbon chain structure of PP itself, the body is not flame retardant and needs to be flame retardant modified.

[0004] Currently, the commonly used high melt strength modification methods include broadening the molecular weight distribution and carbon chain branching technology. Broadening the molecular weight distribution requires the introduction of comonomers such as ethylene, which will reduce the physical properties of the material; materials modified by carbon chain branching technology are easily degraded after screw shearing during post-processing.

[0005] At present, the flame retardant modification technology mainly adopts the method of adding flame retardants. Flame retardants can be divided into halogen-containing flame retardants and halogen-free flame retardants. Common halogen-containing flame retardants include decabromodiphenylethane and octabromoether. Due to their high molecular polarity and incompatibility with the PP matrix, there is a risk of precipitation after long-term use. As people's environmental awareness increases, halogen-containing flame retardants are gradually replaced. Halogen-free flame retardants include intumescent flame retardants, nitrogen-phosphorus powders, etc. To achieve the flame retardant effect, large doses need to be added, and their particle size is generally large, which is not easy to disperse in the PP matrix, and large bubbles will be produced after foaming. Summary of the invention

[0006] The purpose of the present invention is to provide an intrinsic flame retardant polypropylene foam material and a preparation method thereof in view of the deficiencies in the prior art.

[0007] The preparation method of the intrinsic flame-retardant polypropylene foam material of the present invention comprises the following steps: (1) Polypropylene powder, peroxide initiator, and polymerizable monomer A containing both double bonds and isocyanate groups are placed in a ball mill and mixed evenly, and a grafted polymer 1 is obtained by a solid phase grafting method. The ball mill is controlled at a temperature of 80-140° C. and the ball milling time is 0.5-2 h.

[0008] The polypropylene powder is preferably homopolymer polypropylene, and the particle size of the powder is controlled at 1-100 microns. The mass ratio of the polypropylene powder to the peroxide initiator is 100:(0.2-3), and the molar fraction of double bonds in the polymerization monomer A used per 100 g of polypropylene powder is 0.1%-5%.

[0009] The peroxide initiator is selected from the group consisting of dodecyl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, tert-butyl perbenzoate, tert-butyl peroxypivalate, di-tert-butyl peroxide, cumene hydroperoxide, diisopropyl hydroperoxide, parabenzyl hydroperoxide, and bis(2-phenoxyethyl) peroxydicarbonate.

[0010] The polymerizable monomer A is selected from vinyl isocyanate, 3-propylene isocyanate, methacrylate isocyanate, 2-butene isocyanate, styryl isocyanate, isoprene isocyanate, cyclopentene isocyanate, norbornene isocyanate, and methylstyrene isocyanate.

[0011] The principle of obtaining grafted polymer 1 by reaction of polypropylene, peroxide and polymerized monomer A (vinyl isocyanate) is as follows: ; The polypropylene monomers are grafted with isocyanate groups.

[0012] (2) After the grafted polymer 1 and the ungrafted polypropylene powder are mixed in a certain proportion, they are extruded through a twin-screw extruder, and an aminophosphoric acid ester flame retardant is added through a side feeding system in the middle of the extruder. The secondary grafting reaction is carried out by heating and shearing the screw, that is, the amino group of the aminophosphoric acid ester flame retardant reacts with the isocyanate group in the grafted polymer 1 to obtain the grafted polymer 2. The reaction principle is as follows: ; The mass ratio of the polypropylene powder used in step (1) to the ungrafted polypropylene powder used in step (2) is 100:(0-50).

[0013] The aminophosphoric acid ester flame retardant is selected from diphenyl aminophosphoric acid, tris (2-aminoethyl) phosphate, tris (2-hydroxyethyl) aminomethyl phosphate, and diethyl phosphate. The amount of the aminophosphoric acid ester flame retardant is such that the molar ratio of the amino group in the flame retardant to the isocyanate group in the graft polymer is (55-90):100, and the isocyanate group is ensured to be 10%-45% excessive, so as to provide isocyanate groups for the subsequent rigidification reaction.

[0014] (3) The grafted polymer 2 is subjected to a rigidification reaction with excess isocyanate groups through high-temperature steam to obtain polyurea groups, thereby improving the melt strength of the material. The rigidification reaction produces CO2 gas, and the reaction principle is as follows: ; (4) The material obtained in step (3) is subjected to supercritical foaming to obtain an intrinsic flame-retardant polypropylene foam material. The supercritical foaming conditions are preferably: the temperature of the molded foaming cavity is controlled at 140-160°C, the pressure of the supercritical fluid CO2 and / or nitrogen is injected at 8-20 MPa, the temperature and pressure are kept constant for 1-4 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain the foam material.

[0015] The intrinsic flame-retardant polypropylene foam material of the present invention is obtained by adopting the above-mentioned preparation method.

[0016] The advantages of the present invention are: 1. Through ball milling solid phase grafting, the grafting temperature is controlled below the Tm of polypropylene to avoid degradation of polypropylene during high temperature grafting.

[0017] 2. The amino group of aminophosphoric acid ester flame retardant reacts quickly with the isocyanate group in the grafted polymer 1, the grafting efficiency is high in the screw, and there are fewer side reactions.

[0018] 3. The high melt grafting of polypropylene is carried out after the extrusion screw, and the isocyanate and water react on the extrusion line to generate polyurea for hardening. The hardening efficiency is high, and the material will not be sheared by the screw after molding, avoiding the problem of degradation of branched materials. In addition, CO2 will be generated during the hardening process, which provides a gas path for subsequent supercritical foaming and improves the saturation efficiency during supercritical foaming.

[0019] 4. The foaming precursor is foamed by supercritical fluid CO2 and / or nitrogen, and the overall preparation process has the advantages of being clean and environmentally friendly.

[0020] 5. The present invention provides a new flame-retardant polypropylene foam material, which contains both nitrogen and phosphorus elements. The test shows that the halogen-free flame-retardant efficiency is high, and the foam material has excellent physical and mechanical properties. The preparation method of the present invention is novel, which solves the problems of low melt strength and low flame-retardant efficiency of polypropylene. DETAILED DESCRIPTION

[0021] This embodiment is implemented on the premise of the technical solution of the present invention, and provides detailed implementation methods and processes, but the protection scope of the present invention is not limited to the following embodiments. Unless otherwise specified, the materials used are commercially available conventional products.

[0022] In the embodiment, the polypropylene brand used can be T30S, C1608, CP80M, CP80S, EP1X37F, F401, S1004, CF-501, EPS30R, F3002, F400-H, F800E, F800E (DF), FC801, FC801M, FC801MX, JF300, T36F, X37F, X47F, YPF-3003 or YPF-3008. They are all homopolymer polypropylene, and the powder particle size is at 1-100 micron.

[0023] The peroxide initiator is selected from lauryl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, tert-butyl peroxybenzoate, tert-butyl peroxypivalate, di-tert-butyl peroxide, cumene hydroperoxide, diisopropyl hydroperoxide, paraben, bis(2-phenoxyethyl) peroxydicarbonate. Their effects of use are the same, and the embodiments only specifically list some peroxides.

[0024] The polymerizable monomer A is selected from vinyl isocyanate, 3-propylene isocyanate, methacrylic acid isocyanate, 2-butylene isocyanate, styryl isocyanate, isoprene isocyanate, cyclopentene isocyanate, norbornene isocyanate, and methylstyrene isocyanate. They contain both double bonds and isocyanate groups, and have the same effect. Only some of the polymerizable monomers A are listed in the examples.

[0025] The aminophosphoric acid ester flame retardant is selected from diphenyl aminophosphoric acid, tris(2-aminoethyl)phosphate, tris(2-hydroxyethyl)aminomethylphosphate, and diethyl phosphate.

[0026] Example 1 100 g of polypropylene powder, 0.5 g of benzoyl peroxide and 20.7 g of vinyl isocyanate were placed in a ball mill and mixed evenly. The ball mill was controlled at 100°C and the ball milling time was 0.5 h. A grafted polymer 1 was obtained by a solid phase grafting method.

[0027] The obtained grafted 1 polymer and 20 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 54.82 g of diphenyl aminophosphate was added through a side feeding system at the middle position of the extruder. The secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0028] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0029] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 145°C, the pressure of the injected supercritical fluid CO2 is 10 MPa, the temperature and pressure are kept constant for 2 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0030] Example 2 100 g of polypropylene powder, 1.5 g of dodecyl peroxide and 166.2 g of 3-isocyanate propylene were placed in a ball mill and mixed evenly. The ball mill was controlled at 120°C for 1 h to obtain a grafted polymer by a solid phase grafting method.

[0031] The obtained grafted 1 polymer and 30 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 91.84 g of tris(2-aminoethyl)phosphate was added through a side feeding system at the middle position of the extruder. The secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0032] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0033] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 150°C, the pressure of supercritical fluid nitrogen is injected at 15 MPa, the temperature and pressure are kept constant for 3 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0034] Example 3 100 g of polypropylene powder, 3 g of diisopropyl peroxydicarbonate, and 635 g of methyl methacrylate isocyanate were placed in a ball mill and mixed evenly. The ball mill temperature was controlled at 140°C and the ball milling time was 0.8 h. A grafted polymer 1 was obtained by a solid phase grafting method.

[0035] The obtained grafted 1 polymer and 50 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 894 g of tris(2-hydroxyethyl)aminomethyl phosphate was added through a side feeding system at the middle position of the extruder. A secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0036] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0037] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 160°C, the pressure of supercritical fluid nitrogen is injected at 8 MPa, the temperature and pressure are kept constant for 4 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0038] Example 4 100 g of polypropylene powder, 0.2 g of dicyclohexyl peroxydicarbonate, and 13.3 g of styrene isocyanate were placed in a ball mill and mixed evenly. The ball mill was controlled at 80°C for 2 h to obtain a grafted polymer 1 by a solid phase grafting method.

[0039] The obtained grafted 1 polymer and 40 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 10.2 g of diethyl phosphate amine was added through a side feeding system at the middle position of the extruder, and a secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0040] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0041] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 140°C, and the pressure of the supercritical fluid CO2 and supercritical fluid nitrogen mixture injected is 20 MPa. The temperature and pressure are kept constant for 1 hour, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0042] Example 5 100 g of polypropylene powder, 2 g of tert-butyl peroxybenzoate, and 146 g of methyl styrene isocyanate were placed in a ball mill and mixed. The ball mill was controlled at 110°C and the ball milling time was 1.5 h. The grafted polymer 1 was obtained by a solid phase grafting method.

[0043] The obtained graft 1 polymer was extruded through a twin-screw extruder, 198 g of diphenyl aminophosphate was added through a side feeding system at the middle position of the extruder, and a secondary grafting reaction was performed by heating and shearing of the screw to obtain a graft 2 polymer.

[0044] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0045] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 155°C, the pressure of the injected supercritical fluid CO2 is 13 MPa, the temperature and pressure are kept constant for 2.5 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0046] Example 6 100 g of polypropylene powder, 1 g of tert-butyl peroxypivalate, and 440 g of cyclopentene isocyanate were placed in a ball mill and mixed. The ball mill was controlled at 90°C and the ball milling time was 1.8 h. A grafted polymer 1 was obtained by a solid phase grafting method.

[0047] The obtained grafted 1 polymer and 10 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 186 g of tris(2-aminoethyl)phosphate was added through a side feeding system at the middle position of the extruder. A secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0048] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0049] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 145°C, the pressure of the injected supercritical fluid CO2 is 17 MPa, the temperature and pressure are kept constant for 1.5 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0050] Example 7 100 g of polypropylene powder, 2.5 g of cumene hydroperoxide, and 242.5 g of 2-butene isocyanate were placed in a ball mill and mixed. The ball mill temperature was controlled at 130° C. and the ball milling time was 1.2 h. A grafted polymer 1 was obtained by a solid phase grafting method.

[0051] The obtained grafted 1 polymer and 25 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 342.7 g of diphenyl aminophosphate was added through a side feeding system at the middle position of the extruder. A secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0052] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0053] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 150°C, the pressure of supercritical fluid nitrogen is injected at 11 MPa, the temperature and pressure are kept constant for 3.5 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0054] Example 8 100 g of polypropylene powder, 1.2 g of para-methylene hydroperoxide, and 249 g of 3-isocyanate propylene were placed in a ball mill and mixed. The ball mill was controlled at 120° C. for 1 h, and a grafted polymer 1 was obtained by a solid phase grafting method.

[0055] The obtained grafted 1 polymer and 15 g of ungrafted polypropylene powder were mixed and extruded through a twin-screw extruder. 672.8 g of diphenyl aminophosphate was added through a side feeding system at the middle position of the extruder. The secondary grafting reaction was carried out by heating and shearing the screw to obtain a grafted 2 polymer.

[0056] The grafted 2 polymer was subjected to a rigidification reaction with excessive isocyanate groups through high-temperature steam and CO2 gas line establishment, with a speed of 3 m / min and an oven length of 12 m to obtain polyurea groups, which improved the melt strength of the material. The grafted high-melt intrinsic polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0057] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 150°C, the pressure of the injected supercritical fluid CO2 is 14 MPa, the temperature and pressure are kept constant for 3 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain an intrinsic flame-retardant polypropylene foam material.

[0058] Comparative Example 1 100 g of polypropylene powder, 0.5 g of benzoyl peroxide and 20.7 g of vinyl isocyanate were placed in a ball mill and mixed evenly. The ball mill was controlled at 100°C and the ball milling time was 0.5 h. A grafted polymer 1 was obtained by a solid phase grafting method.

[0059] The obtained grafted 1 polymer was mixed with 20 g of ungrafted polypropylene powder and extruded through a twin-screw extruder, and then subjected to rigidification reaction and CO2 gas line establishment through high-temperature steam, with a speed of 3 m / min and an oven length of 12 m. The grafted high-melt polypropylene materials were respectively injection molded into solid sheets with a thickness of 4 mm.

[0060] The solid sheet is subjected to supercritical foaming, the temperature of the molded foaming cavity is controlled at 145°C, the pressure of the injected supercritical fluid CO2 is 10 MPa, the temperature and pressure are kept constant for 2 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain the polypropylene foam material.

[0061] The difference from Example 1 is that no flame retardant grafting is performed.

[0062] Comparative Example 2 100 g of polypropylene powder was extruded through a twin-screw extruder, passed through high-temperature steam, at a speed of 3 m per minute, and an oven length of 12 m, and then the polypropylene materials were injection molded into solid sheets with a thickness of 4 mm. Finally, the solid sheets were subjected to supercritical foaming, the temperature of the molded foaming cavity was controlled at 145°C, the pressure of supercritical fluid CO2 was injected at 10 MPa, the temperature and pressure were kept constant for 2 h, and then the pressure was quickly released at a rate of 1-10 MPa / s. After the pressure was released to normal pressure, the mold was opened to obtain the polypropylene foam material.

[0063] The difference from Example 1 is that no isocyanate group grafting, flame retardant grafting and stiffening reaction were performed.

[0064] Performance Testing The foamed materials prepared in Example 1 and Comparative Examples 1 and 2 were tested according to the horizontal flame retardancy and vertical flame retardancy test methods UL94, tensile strength ASTM-D3574-08, bending measurement method GB-T 8812.2-2007, and surface adhesive strength test GB / T 33332. The results are shown in Table 1.

[0065] Table 1 Test results of foaming materials of Example 1 and Comparative Example 1 and Comparative Example 2

[0066] It can be seen from the test results that Example 1 has a complete two grafting reactions and one rigidification reaction, and a halogen-free flame retardant containing nitrogen and phosphorus elements is grafted on the molecular chain. The solid sheet can pass V-0 vertical combustion, and the flame retardant grade of the material after foaming can reach V-1. Compared with Comparative Example 2, the tensile properties are increased, the melt strength is increased, and the flame retardant properties are increased. In Comparative Example 1, since the raw material still contains nitrogen during the first grafting, the solid sheet still has a certain flame retardant grade. After the rigidification reaction, due to the high content of isocyanate groups in the molecular chain, the rigidification effect is good, the tensile strength and melt strength are higher than those of Example 1, and under the same foaming conditions, the obtained material density is higher. Both Example 1 and Comparative Example 1 have undergone foaming reactions, and there are more bubbles on the surface, so the surface adhesive peeling force shows an upward trend after foaming. Comparative Example 2 did not undergo grafting and rigidification reactions, and its physical and mechanical properties were poor, and it could not meet the melt strength required for supercritical foaming, and the pure material did not have any flame retardant effect.

[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an intrinsic flame retardant polypropylene foam material, characterized in that: The following steps are involved: (1) placing polypropylene powder, a peroxide initiator, and a polymerizable monomer A containing both a double bond and an isocyanate group in a ball mill and mixing them evenly, and obtaining a grafted polymer 1 by a solid phase grafting method; (2) after the grafted 1 polymer and the ungrafted polypropylene powder are mixed in a certain proportion, the mixture is extruded through a twin-screw extruder, an aminophosphoric acid ester flame retardant is added through a side feeding system at the middle of the extruder, and a secondary grafting reaction is performed by heating and shearing the screw, that is, the amino group of the aminophosphoric acid ester flame retardant reacts with the isocyanate group in the grafted 1 polymer to perform grafting, thereby obtaining a grafted 2 polymer; (3) The grafted polymer 2 is subjected to a rigidification reaction with an excess of isocyanate groups through high-temperature steam to obtain polyurea groups, thereby improving the melt strength of the material; (4) The material obtained in step (3) is subjected to supercritical foaming to obtain an intrinsic flame retardant polypropylene foam material.

2. The preparation method according to claim 1, characterized in that: The polypropylene powder is homopolymer polypropylene, and the particle size of the powder is controlled within 1-100 microns.

3. The preparation method according to claim 1, characterized in that: The mass ratio of the polypropylene powder to the peroxide initiator in step (1) is 100:(0.2-3), and the molar fraction of double bonds in the polymerization monomer A used per 100 g of the polypropylene powder is 0.1%-5%.

4. The preparation method according to claim 1, characterized in that: The peroxide initiator in step (1) is selected from the group consisting of dodecyl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, tert-butyl perbenzoate, tert-butyl peroxypivalate, di-tert-butyl peroxide, isopropyl hydroperoxide, diisopropyl hydroperoxide, p-hydroxybenzene hydroperoxide, and bis(2-phenoxyethyl) peroxydicarbonate.

5. The preparation method according to claim 1, characterized in that: The polymerizable monomer A in step (1) is selected from vinyl isocyanate, 3-propylene isocyanate, methacrylate isocyanate, 2-butene isocyanate, styryl isocyanate, isoprene isocyanate, cyclopentene isocyanate, norbornene isocyanate, and methyl styrene isocyanate.

6. The preparation method according to claim 1, characterized in that: The ball mill in step (1) is controlled at a temperature of 80-140° C. and a ball milling time of 0.5-2 h.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the polypropylene powder described in step (1) to the ungrafted polypropylene powder described in step (2) is 100:(0-50).

8. The preparation method according to claim 1, characterized in that: The aminophosphoric acid ester flame retardant in step (2) is selected from diphenyl aminophosphoric acid, tris (2-aminoethyl) phosphate, tris (2-hydroxyethyl) aminomethyl phosphate, and diethyl phosphate amine; the molar ratio of the amino group to the isocyanate group is (55-90):

100.

9. The preparation method according to claim 1, characterized in that: The supercritical foaming conditions in step (4) are as follows: the temperature of the molded foaming cavity is controlled at 140-160°C, the pressure of the injected supercritical fluid CO2 and / or nitrogen is 8-20 MPa, the temperature and pressure are kept constant for 1-4 hours, and then the pressure is quickly released at a rate of 1-10 MPa / s. After the pressure is released to normal pressure, the mold is opened to obtain the foaming material.

10. An intrinsic flame retardant polypropylene foam material, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • High fused mass strength polypropylene containing long branched chain structure and preparing method thereof

    CN101125947A

  • Method for preparing high-melt-strength polypropylene based on solid phase grafting

    CN104356305A

  • Flame retarding agent, flame-retardant aqueous resin composition and flame-retardant urethane resin composition containing said flame retarding agent, and use therefor

    CN104411756A

  • Flame-retardant polypropylene composition, flame-retardant foamed polypropylene and preparation method of flame-retardant foamed polypropylene

    CN112759827A

  • Flame-retardant polymer foam material for automobile and preparation method thereof

    CN116444922A