Carbonizing agent, flame retardant and flame-retardant composite material

The red mud iron tailings are treated by thermosetting resin coating and combining acid and gas sources to prepare flame retardant composite materials, which solves the problems of low utilization rate of red mud iron tailings and environmental pollution, and achieves efficient utilization and flame retardant The performance improvement has promoted the sustainable development of the alumina industry.

CN119060410APending Publication Date: 2024-12-03ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185296.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The utilization rate of red mud iron tailings is low, resulting in land occupation and environmental pollution. The existing technology treatment methods lead to degradation of material performance and difficulty in ensuring stability.

Method used

Carbon agent is prepared by pretreating red mud iron tailings and coating them with thermosetting resin prepolymers to form red mud iron tailings microcapsules, and carbon agent is prepared by combining acid source and gas source. Improve the utilization rate and flame retardant properties of red mud.

Benefits of technology

It has achieved efficient utilization of red mud iron tailings, improved the flame retardant and mechanical properties of the materials, reduced land occupation and environmental pollution, and promoted the sustainable development of the alumina industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060410A_ABST
    Figure CN119060410A_ABST
Patent Text Reader

Abstract

The invention relates to a charring agent, a flame retardant and a flame-retardant composite material. The charring agent is obtained by coating a pretreated red mud iron dressing tailing sample with a thermosetting resin prepolymer. The pretreated red mud iron dressing tailing sample contains a large amount of metal oxides and silicon minerals, can keep a high char yield under a high temperature condition, forms a non-combustible barrier carbon layer in a combustion process, and exerts a solidification phase flame retardant effect; the thermosetting resin has the advantages of high-temperature stability, high mechanical strength, excellent weather resistance and the like; a pretreated red mud iron dressing tailing sample is coated with a thermosetting resin prepolymer, so that the compatibility between the pretreated red mud iron dressing tailing sample and a high-molecular polymer matrix with an inflammable characteristic can be improved, and the protection degree on the polymer matrix is increased; the charring agent can play a synergistic flame-retardant role of thermosetting resin and a pretreated tailing sample during combustion. In conclusion, effective utilization of the red mud iron separation tailings is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of comprehensive utilization of red mud resources, and in particular to a carbonizing agent, a flame retardant and a flame retardant composite material. Background Art

[0002] Alumina production inevitably produces a large amount of red mud. Red mud has a complex composition, usually containing iron oxide, aluminum oxide, silicon oxide and calcium oxide, and may also contain some harmful substances such as heavy metals and radioactive elements. The large amount of red mud not only occupies a large amount of land, but also threatens the health of soil, water and ecosystems, causing serious pollution to the environment.

[0003] According to statistics, red mud has an increasing trend year by year. Faced with the huge pressure of environmental protection and the demand for sustainable development, my country has been actively exploring ways and methods for the resource recycling of red mud for many years to achieve a win-win situation of economic benefits, environmental protection and social sustainable development. Among them, the red mud iron-separation capacity is as high as 8.5 million tons, accounting for 55% of the total utilization, which is an important way to improve the utilization rate of red mud. However, the average yield of iron concentrate in red mud iron-separation is only about 20%. After the red mud is used for iron-separation, a large amount of red mud iron-separation tailings will be produced. The improvement of the utilization rate of red mud is relatively limited, and it will still cause a large amount of land occupation, environmental pollution and other problems. Most of the existing technologies for treating red mud iron-separation tailings directly use them as filling materials. This treatment method will not only cause the performance of the material after filling to deteriorate seriously, but also the stability is difficult to guarantee, and it will cause huge potential harm to the environment. Summary of the invention

[0004] The present application provides a carbon-forming agent, a flame retardant and a flame retardant composite material to solve the following technical problem: how to effectively utilize red mud iron tailings.

[0005] In a first aspect, the present application provides a carbon-forming agent, which is obtained by coating a pretreated red mud iron ore tailings sample with a thermosetting resin prepolymer.

[0006] Optionally, the thermosetting resin includes at least one of the following: phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin, polyurethane resin, and polyester resin.

[0007] Optionally, the pretreated red mud iron ore tailings sample meets the following characteristics: pH value is 8-10, and particle size is greater than 0 mm and not greater than 0.074 mm.

[0008] Optionally, the process parameters of the coating treatment include: a coating temperature of 60° C. to 90° C., and a coating time of 0.5 h to 6 h.

[0009] Optionally, the thermosetting resin prepolymer accounts for 10% to 30% of the weight of the pretreated red mud iron ore tailings sample.

[0010] In a second aspect, the present application provides a flame retardant, wherein the raw material components of the flame retardant include the charring agent described in any one embodiment of the first aspect.

[0011] Optionally, the char-forming agent accounts for 20% to 70% of the weight of the flame retardant.

[0012] Optionally, the raw material components of the carbon-forming agent also include an acid source and a gas source.

[0013] Optionally, the acid source includes at least one of the following: phosphate, borate, sulfate, nitrate; and / or,

[0014] The gas source includes at least one of the following: amino compounds, polyols, amino resins, and carbonates.

[0015] In a third aspect, the present application provides a flame retardant composite material, wherein the flame retardant composite material comprises the flame retardant described in any one embodiment of the second aspect.

[0016] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0017] The carbon-forming agent provided in the embodiment of the present application is obtained by coating a pretreated red mud iron ore tailings sample with a thermosetting resin prepolymer. The pretreated red mud iron ore tailings sample has a large amount of metal oxides and silicon minerals, which can maintain a high carbonization rate under high temperature conditions, form a non-combustible barrier carbon layer during the combustion process, and exert a solid phase flame retardant effect; the thermosetting resin has the advantages of high temperature stability, high mechanical strength and excellent weather resistance; the pretreated red mud iron ore tailings sample is coated with a thermosetting resin prepolymer to obtain a red mud iron ore tailings microcapsule carbonizing agent, which can improve the compatibility of the pretreated red mud iron ore tailings sample with the flammable polymer matrix and increase the degree of protection of the polymer matrix; and the thermosetting resin will release some flame-retardant gases when burning, thereby diluting the concentration of combustible gases and oxygen, and the thermosetting resin and the polymer matrix will quickly cross-link to form a carbon layer, exerting a condensed phase and gas phase flame retardant effect, therefore, the carbonizing agent can exert the synergistic flame retardant effect of the thermosetting resin and the pretreated tailings sample when burning. In summary, the effective utilization of red mud iron ore tailings is achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0020] Figure 1 A microstructure diagram of a melamine resin-coated red mud iron ore tailings microcapsule carbonizing agent provided in an embodiment of the present application;

[0021] Figure 2 A microstructure diagram of a pretreated red mud iron ore tailings sample provided in an embodiment of the present application. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0023] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0024] In this application, the terms "include", "comprises", etc. mean "including but not limited to". In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0026] In a first aspect, the present application provides a carbon-forming agent, which is obtained by coating a pretreated red mud iron ore tailings sample with a thermosetting resin prepolymer.

[0027] In the embodiments of the present application, the pretreated red mud iron ore tailings sample has a large amount of metal oxides and silicon minerals, which can maintain a high carbonization rate under high temperature conditions, form a non-combustible barrier carbon layer during the combustion process, and exert a solid phase flame retardant effect; the thermosetting resin has the following characteristics: high temperature stability, which can form a stable carbonized layer at high temperature, effectively inhibit the spread of flames, and improve the flame retardant properties of the material; high mechanical strength, the carbonized layer formed has high mechanical strength, can resist flame erosion, and protect the substrate from damage; weather resistance, thermosetting resins usually have good weather resistance and can maintain stable performance in harsh environments; designability, by adjusting the formula and process, flame retardant carbonizing agents with different properties can be prepared to meet different application requirements; environmental friendliness, the thermosetting resin flame retardant carbonizing agent has little impact on the environment during production and use, and meets environmental protection requirements. The pretreated red mud iron-draining tailings sample is coated with a thermosetting resin prepolymer to obtain a red mud iron-draining tailings microcapsule carbonizing agent, which can improve the compatibility of the pretreated red mud iron-draining tailings sample with a flammable high molecular polymer matrix and increase the degree of protection of the polymer matrix; and the thermosetting resin will release some non-flammable gas during combustion, thereby diluting the concentration of combustible gas and oxygen, and the thermosetting resin and the polymer matrix will quickly cross-link to form a carbon layer, exerting a condensed phase and gas phase flame retardant effect. Therefore, the carbonizing agent can exert a synergistic flame retardant effect of the thermosetting resin and the pretreated tailings sample during combustion.

[0028] In some embodiments, the thermosetting resin includes at least one of the following: phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin, polyurethane resin, polyester resin.

[0029] In the embodiment of the present application, the thermosetting resin may be phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin,

[0030] One or more of esters, polyurethane resins, and polyester resins, among which melamine resin has good thermal stability, self-extinguishing properties, arc resistance, and good mechanical properties, and has good compatibility with most polymers. Exemplary, Figure 1 A microstructure diagram of a melamine resin-coated red mud iron ore tailings microcapsule carbonizing agent provided in an embodiment of the present application; Figure 2 A microstructure diagram of a pre-treated red mud iron ore tailings sample provided in the embodiment of the present application; see Figures 1-2 It can be seen that the diameter of the uncoated red mud iron tailings pretreatment sample is about 10μm, the particle size distribution is relatively uniform, and the surface is rough. The particle size of the red mud iron tailings microcapsule carbonizing agent coated with melamine resin is about 30μm, and a relatively smooth resin surface is attached to the surface, indicating that the melamine resin is successfully coated to pretreat the red mud iron tailings.

[0031] In some embodiments, the pretreated red mud iron ore tailings sample meets the following characteristics: pH value is 8-10, and particle size is greater than 0 mm and not greater than 0.074 mm.

[0032] In an embodiment of the present application, a method for obtaining a pre-treated red mud iron-draining tailings sample includes: grinding, washing, drying, breaking up, and screening the red mud iron-draining tailings to obtain a pre-treated red mud iron-draining tailings sample.

[0033] The pH value of the pretreated red mud iron tailings sample can be 8 to 10. The reason is that most polymers are sensitive to acidity and alkalinity during high-temperature molding and processing. Too high acidity or alkalinity will affect molding and even cause the polymer to decompose itself. Therefore, the pH value of the pretreated red mud iron tailings sample needs to be controlled to be weakly alkaline. Exemplarily, the pH value of the pretreated red mud iron tailings sample can be 8, 9, 10, etc.

[0034] The particle size of the pretreated red mud iron tailings sample can be greater than 0 mm and not greater than 0.074 mm. On the one hand, it can improve the compatibility of the pretreated red mud iron tailings sample with the flammable polymer matrix and ensure the mechanical properties of the flame-retardant composite material; on the other hand, it can facilitate the subsequent thermosetting resin coating treatment. The coating of high-grade red mud iron tailings is difficult and the coating rate is difficult to ensure. If the particle size is too small, it is not conducive to its dispersion during the coating reaction, resulting in a low coating rate. Exemplary, the particle size can be 0.074 mm, 0.07 mm, 0.06 mm, 0.05 mm, 0.04 mm, etc.

[0035] In some embodiments, the process parameters of the coating treatment include: a coating temperature of 60° C. to 90° C., and a coating time of 0.5 h to 6 h.

[0036] In the embodiment of the present application, the coating temperature of the above coating can be 60° C. to 90° C., and the coating time can be 0.5 h to 6 h.

[0037] The thermosetting resin can be used to coat the pretreated red mud iron tailings sample uniformly, and the coating rate can be guaranteed; if the coating temperature is too high, the resin prepolymer will be cured and polymerized in advance to a certain extent, so that the coating effect cannot be achieved; if the coating temperature is too low or the coating time is too short, it will cause incomplete coating or too low coating rate to a certain extent. If the coating time is too long, the coated red mud iron tailings microcapsule carbonizing agent will agglomerate to a certain extent, making it difficult to disperse, affecting subsequent use. Exemplarily, the coating temperature can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, etc., and the coating time can be 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, etc. Specifically, the pretreated red mud iron tailings sample is mixed with the thermosetting resin prepolymer in a solvent environment, and a chemical reaction occurs in the process parameters of the above-mentioned coating treatment to generate a resin-coated red mud iron tailings microcapsule carbonizing agent. In addition, the solvent for the coating treatment can be one or more of water, ethanol, and methanol. The thermosetting resin prepolymer is prepared in a reaction bottle, and the solvent can be directly added to the reaction bottle to prepare the carbon forming agent in the reaction bottle.

[0038] In some embodiments, the thermosetting resin prepolymer is 10% to 30% by weight of the pretreated red mud iron ore tailings sample.

[0039] In the embodiment of the present application, the thermosetting resin prepolymer can be 10% to 30% of the weight of the pretreated red mud iron tailings sample, which can improve the compatibility of the red mud iron tailings with the flame-retardant composite material, and ensure the low weight loss rate of the red mud iron tailings microcapsule carbonizing agent during the combustion process, ensure a high carbonization rate during the combustion process, and play a solid-phase flame retardant effect. Exemplarily, the above-mentioned thermosetting resin prepolymer can be 10%, 15%, 20%, 25%, 30%, etc. of the weight of the pretreated red mud iron tailings sample.

[0040] In a second aspect, the present application provides a flame retardant, wherein the raw material components of the flame retardant include the charring agent described in any one embodiment of the first aspect.

[0041] The flame retardant is realized based on the above-mentioned charring agent. The specific raw material components of the charring agent can refer to the above-mentioned embodiments. Since the flame retardant adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0042] In some embodiments, the char-forming agent is 20% to 70% by weight of the flame retardant.

[0043] In the embodiment of the present application, the carbonizing agent can be 20% to 70% of the weight of the flame retardant, which can ensure the balance between the formation of the carbon layer and the expansion performance of the flame retardant, and does not affect the physical properties of the material to which it is applied, ensuring that the flame retardant can effectively protect the material under high temperature conditions, while not affecting the performance of the material; if the content of the carbonizing agent is too high, it will cause the carbon layer formed by the flame retardant when heated to be too dense to a certain extent, thereby limiting the expansion, affecting the flame retardant effect, and also destroying the mechanical properties of the flame retardant composite material; if the content of the carbonizing agent is too low, it will cause the carbon layer formed under high temperature conditions to be insufficient to a certain extent, making it difficult to effectively isolate heat, oxygen and combustibles, thereby reducing the flame retardant effect of the flame retardant. Exemplarily, the carbonizing agent can be 20%, 30%, 40%, 50%, 60%, 70%, etc. of the weight of the flame retardant.

[0044] In some embodiments, the raw material components of the char-forming agent further include an acid source and a gas source.

[0045] In the embodiment of the present application, the red mud iron ore tailings microcapsule carbonizing agent forms a stable carbonaceous structure on the polymer surface through its own decomposition and reaction with the polymer matrix when burning and heated, which can not only play the role of heat insulation and oxygen isolation, but also prevent the release of combustible gases and reduce the rate and intensity of combustion. The acid source can provide an acidic environment, promote carbonization reaction, and accelerate the formation of the carbon layer. Under combustion conditions, the acid source decomposes to produce inorganic acids, such as phosphoric acid. These acidic substances can catalyze the dehydration and carbonization of the carbonizing agent to form a protective carbon layer to prevent the flame from spreading further. The acid source can also increase the melting point of the carbon layer, so that it remains stable at high temperatures, prevents molten droplets, and reduces the spread of flames. The gas source can produce difficult or non-combustible gases such as carbon dioxide and water vapor during combustion. These gases form bubbles in the carbon layer, expand the carbon layer, increase its thermal insulation performance, reduce heat transfer, dilute combustible gases, reduce the oxygen concentration in the combustion area, and inhibit combustion. Therefore, the red mud iron tailings microcapsule carbonizing agent, the acid source and the gas source interact and synergistically flame retardant, and together realize the high-efficiency flame retardant performance of the red mud-based intumescent flame retardant. The acid source can be 15% to 65% by weight of the flame retardant; the gas source can be 10% to 60% by weight of the flame retardant. The red mud iron tailings microcapsule carbonizing agent is uniformly mixed with the acid source and the gas source to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0046] In some embodiments, the acid source comprises at least one of: phosphate, borate, sulfate, nitrate; and / or,

[0047] The gas source includes at least one of the following: amino compounds, polyols, amino resins, and carbonates.

[0048] In the embodiments of the present application, the acid source may be one or more of phosphates, borates, sulfates, and nitrates, and the gas source may be one or more of amino compounds, polyols, amino resins, and carbonates.

[0049] In summary, since red mud iron tailings contain metal oxides such as iron and aluminum, as well as flame-retardant, high-carbonization rate silicon minerals, these components can form a stable structure at high temperatures and have good flame retardant properties, which can improve the flame retardancy of materials and reduce fire risks. In addition, the metal oxide components can enhance the mechanical properties of the carbonizing agent, such as hardness and wear resistance, so that it can show better performance in polymers. Therefore, modifying red mud iron tailings to prepare flame-retardant carbonizing agents can not only improve the resource utilization of red mud iron tailings, but also effectively alleviate the problems of land occupation and environmental pressure, which is conducive to improving the utilization rate of red mud and promoting the sustainable development of the alumina industry.

[0050] In a third aspect, the present application provides a flame retardant composite material, wherein the flame retardant composite material comprises the flame retardant described in any one embodiment of the second aspect.

[0051] In the embodiment of the present application, the flame retardant is applied to a high molecular polymer with flammable properties to prepare a flame retardant composite material and the properties of the flame retardant are evaluated by testing. The flame retardant can be 10% to 50% by weight of the flame retardant composite material, which can ensure the balance between the flame retardant properties and the physical properties of the flame retardant composite material, and enable the composite material to have good mechanical properties while ensuring good flame retardant properties. The polymer can be any one of polyoxymethylene, polyurethane, polypropylene, polyvinyl chloride, polyester, polyurethane, polycarbonate, and polyvinyl alcohol.

[0052] A method for preparing a flame-retardant composite material, comprising: uniformly blending a flammable polymer and the flame retardant in a blender, extruding and granulating with a twin-screw extruder, and drying to obtain flame-retardant composite material pellets. The obtained flame-retardant composite material pellets are injection molded in an injection molding machine to obtain an expanded flame-retardant composite material. The extrusion process parameters include: the extrusion temperature can be 160°C to 180°C, and the feeding frequency can be 80Hz to 160Hz. The injection molding process parameters include: the injection molding temperature can be 160°C to 180°C, the injection molding pressure can be 0.20MPa to 0.60MPa, the holding time can be 2s to 10s, and the cooling time can be 10s to 60s.

[0053] The flame retardant composite material meets the following indicators: flame retardant grade no grade ~ V-0 grade, limiting oxygen index 24.7% ~ 40.3%, tensile strength 27.53MPa ~ 39.25MPa, flexural strength 34.68MPa ~ 48.59MPa, notched impact strength 1.95kJ·m -2 ~3.63kJ·m -2 .

[0054] The flame-retardant composite material is realized based on the flame retardant mentioned above. The specific raw material components of the flame retardant can refer to the above embodiments. Since the flame-retardant composite material adopts part or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0055] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0056] Example 1

[0057] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a melamine resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 80° C., the coating time is 1 hour, the coating solvent is an ethanol aqueous solution, and the melamine resin is 1 / 9 of the weight of the pretreated red mud iron-separation tailings sample.

[0058] A method for preparing a carbonizing agent comprises: reacting 45g of a pretreated red mud iron tailing sample with 5g of a melamine resin prepolymer in an ethanol aqueous solution at 80°C for 1h, and then filtering and drying to obtain 50g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0059] Specifically, 45g of red mud iron-selected tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-selected tailings sample. 5.63g of 37wt% formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, heated to 60°C and kept at a constant temperature, 2.92g of melamine was added, and the melamine resin prepolymer was obtained after constant temperature reaction for 1h, and then 7.1mL of ethanol was directly added to the reaction bottle, the temperature was raised to 80°C, and 45g of the pretreated red mud iron-selected tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 1h, filtered, dried, and 50g of resin-coated red mud iron-selected tailings microcapsule carbonizing agent was obtained.

[0060] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0061] Specifically, 50 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0062] A flame retardant composite material comprises: polyoxymethylene and a flame retardant; 350g of polyoxymethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 170°C, the feeding frequency is 160Hz, the injection molding temperature is 170°C, the injection molding pressure is 0.30MPa, the holding time is 2s, and the cooling time is 10s.

[0063] Example 2

[0064] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a melamine resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 80° C., the coating time is 1 hour, the coating solvent is an ethanol aqueous solution, and the melamine resin is 1 / 9 of the weight of the pretreated red mud iron-separation tailings sample.

[0065] A method for preparing a carbonizing agent comprises: reacting 90g of a pretreated red mud iron tailing sample with 10g of a melamine resin prepolymer in an ethanol aqueous solution at 80°C for 1h, and then filtering and drying to obtain 100g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0066] Specifically, 90g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample. 11.26g of 37wt% formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, heated to 60°C and kept at a constant temperature, 5.83g of melamine was added, and the melamine resin prepolymer was obtained after constant temperature reaction for 1h, 14.2mL of ethanol was added to the reaction bottle, the temperature was raised to 80°C, and 90g of the pretreated red mud iron-separation tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 1h, filtered, dried, and 100g of resin-coated red mud iron-separation tailings microcapsule carbonizing agent was obtained.

[0067] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0068] Specifically, 100 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0069] A flame retardant composite material comprises: polyoxymethylene and a flame retardant; 300g of polyoxymethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 175°C, the feeding frequency is 120Hz, the injection molding temperature is 175°C, the injection molding pressure is 0.40MPa, the holding time is 5s, and the cooling time is 20s.

[0070] Example 3

[0071] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a melamine resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 80° C., the coating time is 2 hours, the coating solvent is an ethanol aqueous solution, and the melamine resin is 1 / 4 of the weight of the pretreated red mud iron-separation tailings sample.

[0072] A method for preparing a carbonizing agent comprises: reacting 80g of a pretreated red mud iron tailing sample with 20g of a melamine resin prepolymer in an ethanol aqueous solution at 80°C for 2h, and then filtering and drying to obtain 100g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0073] Specifically, 80g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample. 22.52g of 37wt% formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, heated to 60°C and kept at a constant temperature, 11.67g of melamine was added, and the melamine resin prepolymer was obtained after constant temperature reaction for 1h, 28.4mL of ethanol was added to the reaction bottle, the temperature was raised to 80°C, and 80g of the pretreated red mud iron-separation tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 2h, filtered, dried, and 100g of resin-coated red mud iron-separation tailings microcapsule carbonizing agent was obtained.

[0074] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0075] Specifically, 100 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0076] A flame retardant composite material comprises: polyoxymethylene and a flame retardant; 300g of polyoxymethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 175°C, the feeding frequency is 120Hz, the injection molding temperature is 175°C, the injection molding pressure is 0.40MPa, the holding time is 5s, and the cooling time is 20s.

[0077] Example 4

[0078] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a melamine resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 80° C., the coating time is 1 hour, the coating solvent is an ethanol aqueous solution, and the melamine resin is 1 / 9 of the weight of the pretreated red mud iron-separation tailings sample.

[0079] A method for preparing a carbonizing agent comprises: reacting 135g of a pretreated red mud iron tailing sample with 15g of a melamine resin prepolymer in an ethanol aqueous solution at 80°C for 1h, and then filtering and drying to obtain 150g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0080] Specifically, 135g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample. 16.89g of 37wt% formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, heated to 60°C and kept at a constant temperature, 8.75g of melamine was added, and the melamine resin prepolymer was obtained after constant temperature reaction for 1h, 21.3mL of ethanol was added to the reaction bottle, the temperature was raised to 80°C, and 135g of the pretreated red mud iron-separation tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 1h, filtered, dried, and 150g of resin-coated red mud iron-separation tailings microcapsule carbonizing agent was obtained.

[0081] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0082] Specifically, 150 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0083] A flame retardant composite material comprises: polyoxymethylene and a flame retardant; 250g of polyoxymethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 180°C, the feeding frequency is 80Hz, the injection molding temperature is 180°C, the injection molding pressure is 0.45MPa, the holding time is 8s, and the cooling time is 30s.

[0084] Example 5

[0085] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a melamine resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 80° C., the coating time is 2 hours, the coating solvent is an ethanol aqueous solution, and the melamine resin is 1 / 4 of the weight of the pretreated red mud iron-separation tailings sample.

[0086] A method for preparing a carbonizing agent comprises: reacting 120g of a pretreated red mud iron tailing sample with 30g of a melamine resin prepolymer in an ethanol aqueous solution at 80°C for 2h, and then filtering and drying to obtain 150g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0087] Specifically, 120g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample. 33.78g of formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, heated to 60°C and kept at a constant temperature, 17.50g of melamine was added, and the melamine resin prepolymer was obtained after constant temperature reaction for 1h, 42.6mL of ethanol was added to the reaction bottle, the temperature was raised to 80°C, and 120g of the pretreated red mud iron-separation tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 2h, filtered, dried, and 150g of resin-coated red mud iron-separation tailings microcapsule carbonizing agent was obtained.

[0088] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0089] Specifically, 150 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0090] A flame retardant composite material comprises: polyoxymethylene and a flame retardant; 250g of polyoxymethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 180°C, the feeding frequency is 80Hz, the injection molding temperature is 180°C, the injection molding pressure is 0.45MPa, the holding time is 8s, and the cooling time is 30s.

[0091] Example 6

[0092] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a phenolic resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 75° C., the coating time is 1.5 hours, the coating solvent is an aqueous solution, and the phenolic resin is 1 / 4 of the weight of the pretreated red mud iron-separation tailings sample.

[0093] A method for preparing a carbonizing agent comprises: reacting 120g of a pretreated red mud iron tailing sample with 30g of a phenolic resin prepolymer in an ethanol aqueous solution at 75°C for 1.5h, and then filtering and drying to obtain 150g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0094] Specifically, 120g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample. 15.89g of formaldehyde aqueous solution and 30mL of deionized water were added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, and a constant temperature of 25°C was maintained, and 27.64g of phenol was added. After isothermal reaction for 1h, a phenolic resin prepolymer was obtained, and the temperature was raised to 80°C, and 120g of the pretreated red mud iron-separation tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 1.5h, filtered, dried, and 150g of resin-coated red mud iron-separation tailings microcapsule carbonizing agent was obtained.

[0095] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0096] Specifically, 150 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0097] A flame retardant composite material comprises: polypropylene and a flame retardant; 250g of polypropylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polypropylene pellets. The obtained flame retardant polypropylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polypropylene composite material. The extrusion temperature is 180°C, the feeding frequency is 90Hz, the injection molding temperature is 180°C, the injection molding pressure is 0.45MPa, the holding time is 10s, and the cooling time is 30s.

[0098] Example 7

[0099] A carbon-forming agent is obtained by coating a pretreated red mud iron-separation tailings sample with a urea-formaldehyde resin prepolymer, wherein the pH value of the pretreated red mud iron-separation tailings sample is 10, the particle size is greater than 0 mm and not greater than 0.074 mm, the coating temperature is 70° C., the coating time is 1 hour, the coating solvent is a methanol aqueous solution, and the urea-formaldehyde resin is 1 / 4 of the weight of the pretreated red mud iron-separation tailings sample.

[0100] A method for preparing a carbonizing agent comprises: reacting 120g of a pretreated red mud iron tailing sample with 30g of a urea-formaldehyde resin prepolymer in a 70°C methanol aqueous solution for 1h, and then filtering and drying to obtain 150g of a resin-coated red mud iron tailing microcapsule carbonizing agent.

[0101] Specifically, 120g of red mud iron-selected tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-selected tailings sample. 47.69g of formaldehyde aqueous solution was added to a reaction bottle, and the pH value of the reaction solution was adjusted to 9 with a 10wt% sodium carbonate aqueous solution, and a constant temperature of 25°C was maintained, and 17.64g of urea was added, and the urea-formaldehyde resin prepolymer was obtained after constant temperature reaction for 1h, and 56.0mL of methanol was added to the reaction bottle, and the temperature was raised to 70°C, and then 120g of the pretreated red mud iron-selected tailings sample was added to the reaction bottle and continued to be stirred at a constant temperature for 2h, filtered, dried, and 150g of resin-coated red mud iron-selected tailings microcapsule carbonizing agent was obtained.

[0102] A flame retardant comprises: a red mud iron ore tailing microcapsule carbonizing agent, an acid source and a gas source; the acid source is ammonium polyphosphate, and the gas source is melamine.

[0103] Specifically, 150 g of the prepared resin-coated red mud iron ore tailings microcapsule carbonizing agent is evenly mixed with 75 g of ammonium polyphosphate and 25 g of melamine to obtain a green and environmentally friendly red mud-based intumescent flame retardant.

[0104] A flame retardant composite material, comprising: polyethylene and a flame retardant; 250g of polyethylene and the flame retardant are uniformly blended in a blender, then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyethylene pellets. The obtained flame retardant polyethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyethylene composite material. The extrusion temperature is 175°C, the feeding frequency is 100Hz, the injection molding temperature is 175°C, the injection molding pressure is 0.45MPa, the holding time is 10s, and the cooling time is 30s.

[0105] Comparative Example 1

[0106] A flame retardant composite material, comprising: 75g of ammonium polyphosphate, 25g of melamine, and 400g of polyoxymethylene are uniformly blended in a blender, and then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 160°C, the feeding frequency is 160Hz, the injection molding temperature is 160°C, the injection molding pressure is 0.20MPa, the holding time is 2s, and the cooling time is 10s.

[0107] Comparative Example 2

[0108] A flame retardant composite material, comprising: 30g of melamine resin, 75g of ammonium polyphosphate, 25g of melamine, and 370g of polyoxymethylene are uniformly blended in a blender, and then extruded and granulated by a twin-screw extruder, and dried to obtain flame retardant polyoxymethylene pellets. The obtained flame retardant polyoxymethylene pellets are injection molded in an injection molding machine to obtain an expanded flame retardant polyoxymethylene composite material. The extrusion temperature is 165°C, and the feeding frequency is 160Hz. The injection molding temperature is 165°C, the injection molding pressure is 0.30MPa, the holding time is 2s, and the cooling time is 20s.

[0109] Comparative Example 3

[0110] 120 g of red mud iron-separation tailings were ground and washed until the pH value of the washing water dropped to 10, filtered, dried, and broken up, and passed through a 200-mesh sieve to obtain a pretreated red mud iron-separation tailings sample.

[0111] 120g of pretreated red mud iron tailings sample was mixed evenly with 30g of melamine resin, 75g of melamine, 25g of melamine and 250g of polyoxymethylene in a blender, and then extruded and granulated by a twin-screw extruder, and dried to obtain flame-retardant polyoxymethylene pellets. The obtained flame-retardant polyoxymethylene pellets were injection molded in an injection molding machine to obtain an expanded flame-retardant polyoxymethylene composite material. Among them, the extrusion temperature was 180°C and the feeding frequency was 80Hz. The injection molding temperature was 180°C, the injection molding pressure was 0.60MPa, the holding time was 10s, and the cooling time was 40s.

[0112] Comparative Example 4

[0113] 150g of pentaerythritol, 75g of ammonium polyphosphate, 25g of melamine and 250g of polyoxymethylene were uniformly blended in a blender, and then extruded and granulated using a twin-screw extruder. Flame-retardant polyoxymethylene pellets were obtained after drying. The obtained flame-retardant polyoxymethylene pellets were injection molded in an injection molding machine to obtain an expanded flame-retardant polyoxymethylene composite material. The extrusion temperature was 180°C, the feeding frequency was 80Hz, the injection molding temperature was 180°C, the injection molding pressure was 0.60MPa, the holding time was 10s, and the cooling time was 60s.

[0114] The intumescent flame-retardant composite materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4 were compared and analyzed, and the results are shown in Table 1.

[0115] Table 1 Flame retardant and mechanical properties data of flame retardant composite materials

[0116]

[0117] As can be seen from Table 1, the intumescent flame-retardant composite materials of Examples 1 to 7 all have the advantages of good processability and good thermal stability. By comparing the test data of Example 5 with that of Comparative Example 1, it can be found that the introduction of 20% resin-coated red mud iron-separation tailings microcapsule carbonizing agent greatly improves the flame retardant properties of the composite material, the vertical combustion grade is increased from no grade to the highest grade V-0, and the limiting oxygen index is greatly increased from 22.6% to 40.3%. It can be obtained that the red mud-based intumescent flame retardant prepared by compounding 20% ​​resin-coated red mud iron-separation tailings microcapsule carbonizing agent with ammonium polyphosphate and melamine can play a good flame retardant effect in the polyoxymethylene matrix. However, due to the introduction of a large amount of red mud iron-separation tailings microcapsule carbonizing agent, the composite material suffers from partial loss of mechanical properties.

[0118] By comparing the test data of Example 5 with that of Comparative Example 2, it can be found that, judging only from the flame retardant effect, the red mud iron tailings microcapsule carbonizing agent component that plays a major role in the flame retardant effect of the composite material should be the red mud iron tailings, rather than the melamine resin coated on the surface of the red mud iron tailings.

[0119] By comparing the test data of Example 5 with that of Comparative Example 3, it can be found that the mechanical properties of the composite material in Example 5 have been comprehensively improved, and the tensile strength, flexural strength and notched impact strength have been improved by 38.7%, 43.0% and 29.3%, respectively. This is because the red mud iron tailings that have not been coated with melamine resin have poor compatibility with the polyoxymethylene matrix, and a large amount of introduction is bound to cause great losses to the mechanical properties of the composite material; the compatibility of the red mud iron tailings coated with melamine resin and the polyoxymethylene matrix has been improved, which makes up for the loss of mechanical properties of some composite materials. In addition, since the red mud iron tailings that have not been coated with melamine resin have poor compatibility in the polyoxymethylene matrix, it is difficult to ensure its dispersibility during mixing and processing, so the flame retardant properties of the composite material in Comparative Example 3 are slightly lower than those in Example 5.

[0120] By comparing the test data of Example 5 with that of Comparative Example 4, it can be found that the most commonly used intumescent flame retardants (ammonium polyphosphate, melamine, pentaerythritol) on the market are used in polyoxymethylene matrix, and the vertical burning test does not reach any flame retardant level, and the limiting oxygen index is only 31.7%. The red mud-based intumescent flame retardant performs relatively well in terms of flame retardancy and mechanical properties, wherein the vertical burning grade reaches V-0, and the limiting oxygen index is as high as 40.3%. The mechanical properties have also been comprehensively improved, wherein the tensile strength, flexural strength and notched impact strength have been improved by 28.6%, 37.9% and 19.3% respectively. The red mud-based intumescent flame retardant exhibits excellent flame retardancy.

[0121] The test data of Example 6 and Example 7 show that the red mud iron tailings microcapsule carbonizing agent prepared by coating with different resins exhibits good flame retardant properties in polymer matrices with different flammable properties, and does not cause huge loss of mechanical properties of the composite material.

[0122] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0123] (1) In the embodiment of the present application, the red mud iron ore tailings microcapsule carbonizing agent is prepared by coating the pretreated red mud iron ore tailings with a thermosetting resin prepolymer, which exhibits good flame retardant properties in a flammable polymer matrix without causing a huge loss in mechanical properties of the composite material;

[0124] (2) By preparing green and environmentally friendly red mud iron tailings microcapsule carbonizing agent, the green and efficient utilization of red mud iron tailings can be achieved, alleviating the prominent problems of land occupation and environmental pollution caused by red mud iron tailings in my country. It can also greatly increase the value of red mud iron tailings and realize the green high added value transformation of red mud iron tailings.

[0125] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A carbon-forming agent, characterized in that The carbon-forming agent is obtained by coating a pretreated red mud iron ore tailing sample with a thermosetting resin prepolymer.

2. The carbon-forming agent according to claim 1, characterized in that The thermosetting resin includes at least one of the following: phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin, polyurethane resin, and polyester resin.

3. The carbon-forming agent according to claim 1, characterized in that The pretreated red mud iron ore tailings sample meets the following characteristics: a pH value of 8 to 10, and a particle size of greater than 0 mm and not greater than 0.074 mm.

4. The carbon-forming agent according to claim 1, characterized in that The process parameters of the coating treatment include: coating temperature of 60° C. to 90° C., and coating time of 0.5 h to 6 h.

5. The carbon-forming agent according to any one of claims 1 to 4, characterized in that: The thermosetting resin prepolymer accounts for 10% to 30% of the weight of the pretreated red mud iron ore tailings sample.

6. A flame retardant, characterized in that: The raw material components of the flame retardant include the charring agent according to any one of claims 1 to 5.

7. The flame retardant according to claim 6, characterized in that The carbon-forming agent accounts for 20% to 70% of the weight of the flame retardant.

8. The flame retardant according to claim 6, characterized in that The raw material components of the carbon-forming agent also include an acid source and a gas source.

9. The flame retardant according to claim 8, characterized in that The acid source comprises at least one of the following: phosphate, borate, sulfate, nitrate; and / or, The gas source includes at least one of the following: amino compounds, polyols, amino resins, and carbonates.

10. A flame retardant composite material, characterized in that: The flame retardant composite material comprises the flame retardant according to any one of claims 6 to 9.