High-wear-resistance rubber material for charging cable of automobile charging pile and preparation method of high-wear-resistance rubber material

Through the combination of hydrogenated nitrile rubber and modified polyetherimide blend crosslinking system and nanofiller, the problem of insufficient wear resistance and heat resistance of traditional charging pile cable materials is solved, and an excellent mechanical and electrical performance is prepared The rubber for charging cables of high wear-resistant automobile charging piles ensures stable use in high voltage environments.

CN119060431APending Publication Date: 2024-12-03TAICANG GUANLIAN POLYMERIC MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410990013.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional charging pile cable materials are difficult to meet the requirements of wear resistance, heat resistance, ultraviolet resistance, etc., and are prone to aging and cracking, affecting service life and safety, especially in high voltage and high current environments.

Method used

Hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) are used to blend crosslinking system, and nanofillers, plasticizers and assisted crosslinking agents are introduced to prepare high resistance through twin-screw kneading and dynamic vulcanization processes. Grind the rubber for charging cables for car charging piles.

Benefits of technology

It improves the wear resistance, heat resistance, mechanical properties and electrical insulation properties of the rubber, can maintain stability in high voltage environments, extend the service life of charging pile cables and improve safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of cable sizing materials, in particular to a high-wear-resistance sizing material for a charging cable of an automobile charging pile and a preparation method of the high-wear-resistance sizing material. The invention discloses a high-wear-resistance rubber material for a charging cable of an automobile charging pile. The high-wear-resistance rubber material is prepared from the following raw material components in parts by mass: 50-70 parts of hydrogenated nitrile rubber (HNBR), 10-20 parts of modified polyetherimide (PEI), 5-10 parts of nano filler, 5-10 parts of a plasticizer, 1.5-3.5 parts of an assistant crosslinking agent and 2.0-5.0 parts of a vulcanizing agent. HNBR (hydrogenated nitrile butadiene rubber) and PEI (modified polyetherimide) are adopted to blend a cross-linking system; polyetherimide (PEI) is grafted and modified through a silane coupling agent, so that the compatibility of the PEI and HNBR interface bonding can be improved; due to the introduction of the nano filler, the interface area is increased, the interface interaction is enhanced, meanwhile, physical cross-linking points are formed, and the cross-linking points can resist the action of external friction force, so that the wear resistance and the thermal stability of the composite material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cable rubber materials, and in particular to a highly wear-resistant rubber material for a charging cable of a vehicle charging pile and a preparation method thereof. Background Art

[0002] Traditional charging pile cable materials often fail to meet the requirements of wear resistance, heat resistance, and UV resistance, and are prone to problems such as aging and cracking, which affects the service life and safety of the charging pile.

[0003] There are obvious differences between new energy vehicle cables and traditional vehicle cables. Due to the particularity of the use environment, new energy vehicle cables need to cope with high voltage and high current situations. For example, the vehicle voltage can reach 600-800V, while the battery voltage of traditional fuel vehicles is generally 12-24V. Car charging cables also need to have excellent voltage resistance to cope with high voltage and high current working conditions.

[0004] At present, some research institutions and enterprises at home and abroad have begun to develop high-wear-resistant rubber materials for electric vehicle charging pile charging cables, and have achieved certain results. For example, some enterprises have adopted new polymer materials and additives to improve the wear resistance and heat resistance of rubber materials; some research institutions have improved the comprehensive performance of rubber materials by optimizing the formula and production process. Summary of the invention

[0005] Technical problem to be solved: In order to overcome the above-mentioned shortcomings, a highly wear-resistant rubber compound for automobile charging pile charging cables and a preparation method thereof are provided; this rubber compound needs to have good wear resistance, heat resistance, voltage resistance, and good mechanical properties to ensure the long-term and stable use of the charging pile cables.

[0006] The technical solution is: a highly wear-resistant rubber compound for automobile charging pile charging cables, comprising the following raw material components in parts by mass: 50-70 parts of hydrogenated nitrile rubber (HNBR), 10-20 parts of modified polyetherimide (PEI), 5-10 parts of nanofiller, 5-10 parts of plasticizer, 1.5-3.5 parts of co-crosslinking agent, and 2.0-5.0 parts of vulcanizing agent.

[0007] Preferably, the preparation process of the modified polyetherimide comprises the following steps:

[0008] Step 1) Clean the PEI sample with ethanol or acetone to remove surface impurities and oil stains, and then dry it at 60-80° C. to ensure that there is no moisture on the surface;

[0009] Step 2) dissolving an appropriate amount of silane coupling agent (such as 3-aminopropyltriethoxysilane, APTES) in anhydrous ethanol to prepare a 0.5-2% solution, stirring evenly to ensure that the silane coupling agent is completely dissolved;

[0010] Step 3) immersing the dried PEI sample in a silane coupling agent solution for 30-60 minutes to ensure that the silane coupling agent reacts fully with the PEI surface, and stirring slightly during the immersion process to improve the treatment effect;

[0011] Step 4) Take out the treated PEI sample, wash it with anhydrous ethanol or deionized water to remove the unreacted silane coupling agent; then dry it at 60-80° C. to ensure that there is no residual solvent on the surface.

[0012] Step 5) curing the dried PEI sample at 120-150° C. for 1-2 hours to ensure that the silane coupling agent forms a stable chemical bond on the surface of PEI, thereby obtaining modified polyetherimide.

[0013] Preferably, the nanofiller is nano-silicon dioxide or nano-aluminum oxide.

[0014] Preferably, the plasticizer is any one of dioctyl adipate (DOA) and dioctyl sebacate (DOS), or a combination of both.

[0015] Preferably, the auxiliary cross-linking agent is TAIC or TAC, or a combination of both.

[0016] Preferably, the vulcanizing agent is any one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane or bis-(tert-butylperoxyisopropyl)benzene, or a combination of both.

[0017] The preparation method of the highly wear-resistant rubber material for automobile charging pile charging cable is as follows:

[0018] 1) All raw materials are weighed accurately by mass, and hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) are preliminarily mixed at room temperature to ensure that the two are evenly distributed.

[0019] 2) Add the pre-mixed HNBR and PEI mixture into a twin-screw mixer, and gradually add nanofiller, plasticizer, co-crosslinking agent and vulcanizing agent. The mixer temperature is set to 150-180°C and the speed is controlled at 100-200rpm. Maintain uniform mixing during the mixing process to ensure that all components are fully dispersed.

[0020] 3) Dynamic vulcanization is carried out in the rear section of the twin-screw mixer, the vulcanization temperature is set to 180-200°C, and the vulcanization time is 5-10 minutes.

[0021] 4) The mixture extruded from the twin-screw mixer is rapidly cooled by a cooling device to obtain the desired rubber compound.

[0022] Beneficial effects: 1. Hydrogenated nitrile rubber (HNBR) has good wear resistance, and modified polyetherimide (PEI) has good heat resistance. The cross-linking system of hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) is adopted. The polyetherimide (PEI) is grafted with a silane coupling agent to improve its compatibility with the HNBR interface. The introduction of nanofillers increases the interface area, enhances the interface interaction, and forms physical cross-linking points at the same time. These cross-linking points can resist the effect of external friction, thereby improving the wear resistance and thermal stability of the composite material.

[0023] 2. Both hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) have good electrical insulation properties; and the introduction of nanofillers can fill the gaps and defects in the rubber matrix to form a denser insulating structure, which makes the composite materials after their blending able to resist high voltage corrosion.

[0024] 3. By rationally selecting and proportioning the components, and utilizing twin-screw mixing and dynamic vulcanization processes, the components are fully mixed and cross-linked to form a rubber compound with excellent physical and mechanical properties. DETAILED DESCRIPTION

[0025] The present invention is described in detail below with reference to specific embodiments, but is not intended to limit the present invention.

[0026] A highly wear-resistant rubber compound for a charging cable of a car charging pile comprises the following raw material components in parts by mass: 50-70 parts of hydrogenated nitrile rubber (HNBR), 10-20 parts of modified polyetherimide (PEI), 15-20 parts of nano filler, 5-10 parts of plasticizer, 1.5-3.5 parts of co-crosslinking agent, and 2.0-5.0 parts of vulcanizing agent.

[0027] Hydrogenated nitrile rubber (HNBR) itself converts most of the unsaturated bonds (such as carbon-carbon double bonds) into saturated bonds through hydrogenation reaction, thereby improving the rigidity and cohesion of the rubber's molecular chain, enabling it to withstand greater friction and wear.

[0028] The saturated structure of hydrogenated nitrile rubber (HNBR) gives it excellent heat resistance. Due to the reduction of unsaturated bonds, HNBR is not prone to oxidation, degradation and other reactions at high temperatures, thus maintaining good physical and heat resistance.

[0029] When HNBR is blended with modified polyetherimide (PEI), the interfacial compatibility between the two is improved due to the grafting effect of the silane coupling agent, so that the composite material can form a more stable interface structure when subjected to friction, further enhancing the physical and mechanical properties of the composite material.

[0030] Both hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) have good electrical insulation properties; the introduction of nanofillers can fill the gaps and defects in the rubber matrix to form a denser insulation structure, which makes the composite material after blending them resistant to high voltage corrosion.

[0031] Preferably, the preparation process of the modified polyetherimide comprises the following steps:

[0032] Step 1) Clean the PEI sample with ethanol or acetone to remove surface impurities and oil stains, and then dry it at 60-80° C. to ensure that there is no moisture on the surface;

[0033] Step 2) dissolving an appropriate amount of silane coupling agent (such as 3-aminopropyltriethoxysilane, APTES) in anhydrous ethanol to prepare a 0.5-2% solution, stirring evenly to ensure that the silane coupling agent is completely dissolved;

[0034] Step 3) immersing the dried PEI sample in a silane coupling agent solution for 30-60 minutes to ensure that the silane coupling agent reacts fully with the PEI surface, and stirring slightly during the immersion process to improve the treatment effect;

[0035] Step 4) Take out the treated PEI sample, wash it with anhydrous ethanol or deionized water to remove the unreacted silane coupling agent; then dry it at 60-80° C. to ensure that there is no residual solvent on the surface.

[0036] Step 5) The dried PEI sample is cured at 120-150° C. for 1-2 hours to ensure that the silane coupling agent forms a stable chemical bond on the PEI surface.

[0037] In the specific implementation process, the nanofiller is nano-silicon dioxide or nano-aluminum oxide; the nanofiller has a very large specific surface area due to its extremely small size. When the nanofiller is dispersed in the polymer matrix, the interface area of ​​the two materials can be significantly increased, thereby enhancing the interface interaction. At the same time, the nanofiller can form physical crosslinking points in the polymer matrix, increasing the crosslinking density of the material, and these physical crosslinking points can improve the mechanical properties and thermal stability of the material.

[0038] In the specific implementation process, the plasticizer is any one of dioctyl adipate (DOA) or dioctyl sebacate (DOS) or both. DOA and DOS can be used in the rubber compound to give the rubber compound excellent cold resistance. DOS is very suitable for the situation where both heat resistance and low temperature resistance are required.

[0039] In a specific implementation process, the auxiliary cross-linking agent is any one of TAIC or TAC or a combination of both.

[0040] In a specific implementation process, the vulcanizing agent is any one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane or bis-(tert-butylperoxyisopropyl)benzene, or a combination of both.

[0041] The preparation method of the highly wear-resistant rubber material for automobile charging pile charging cable is as follows:

[0042] 1) All raw materials are weighed accurately by mass, and hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) are preliminarily mixed at room temperature to ensure that the two are evenly distributed.

[0043] 2) Add the pre-mixed HNBR and PEI mixture into a twin-screw mixer, and gradually add nanofiller, plasticizer, co-crosslinking agent and vulcanizing agent. The mixer temperature is set to 150-180°C and the speed is controlled at 100-200rpm. Maintain uniform mixing during the mixing process to ensure that all components are fully dispersed.

[0044] 3) Dynamic vulcanization is carried out in the rear section of the twin-screw mixer, the vulcanization temperature is set to 180-200°C, and the vulcanization time is 5-10 minutes.

[0045] 4) The mixture extruded from the twin-screw mixer is rapidly cooled by a cooling device to obtain the desired rubber compound.

[0046] In the specific implementation process, the raw material components and proportions of the rubber material for a highly wear-resistant automobile charging pile charging cable prepared in Examples 1-4 and Comparative Examples 1-2 are shown in Table 1 below:

[0047]

[0048] Trial plan

[0049] Hardness test: Use Shore A durometer to measure the hardness of the rubber, the range is between 70-80 Shore A.

[0050] Tensile strength and elongation at break test: Tensile test is carried out under standard conditions to measure tensile strength (≥8MPa) and elongation at break (≥250%)

[0051] Hot air aging test: Aging at 135℃ for 168 hours, measuring the change rate of tensile strength and elongation, requiring the change rate to be within ±25%. Low temperature brittleness test: Keep at -40℃ for 3 minutes, check whether the sample has cracks, requiring no cracks.

[0052] Volume resistivity test: Measure volume resistivity at 20°C, requirement ≥4.0*10 13 Ω*cm. Roller abrasion test: measure the abrasion of rubber, requirement ≤300mm 3 .

[0053] Data Analysis:

[0054] The performance parameters of the rubber materials prepared in Examples 1-4 and Comparative Examples 1-2 are shown in Table 2 below:

[0055]

[0056]

[0057] From the data analysis in Table 2, it can be seen that in the performance parameter test data of Examples 1-4, Comparative Example 1 (unmodified polyetherimide (PEI)) and Comparative Example 2 (no nanofiller added), the key performance parameters such as hardness, tensile strength, and elongation at break of Examples 1-4 are all better than those of Comparative Examples 1-2.

[0058] Especially in terms of performance retention after hot air aging, the rubber materials prepared in Examples 1-4 showed more significant stability. It was confirmed that the grafting modification of PEI by combining silane coupling agent in Examples 1-4 significantly improved the interfacial compatibility between HNBR and PEI; this improvement not only enhanced the bonding force between the two materials. The introduction of nanofillers not only increased the interfacial area and enhanced the interfacial interaction, but also greatly improved the mechanical properties and thermal stability of the composite material by forming physical crosslinking points.

[0059] The above performance characteristics indicate that the present invention has good wear resistance, voltage resistance, aging resistance, cold resistance and other characteristics. By reasonably adjusting the formula and process parameters, rubber materials that meet different application requirements can be prepared, providing high-performance material options for fields such as automobile charging piles and charging cables.

[0060] The above embodiments are provided for persons familiar with the art to implement or use the present invention. Personnel familiar with the art can make various modifications or changes to the above embodiments without departing from the inventive concept of the present invention. Therefore, the protection scope of the present invention is not limited to the above embodiments, but should be the maximum scope of the innovative features mentioned in the claims.

Claims

1. A highly wear-resistant rubber compound for automobile charging pile charging cables, characterized in that: The invention comprises the following raw material components in parts by mass: 50-70 parts of hydrogenated nitrile rubber (HNBR), 10-20 parts of modified polyetherimide (PEI), 5-10 parts of nano filler, 5-10 parts of plasticizer, 1.5-3.5 parts of auxiliary cross-linking agent and 2.0-5.0 parts of vulcanizing agent.

2. The highly wear-resistant rubber material for automobile charging pile charging cable according to claim 1, characterized in that: The preparation process of the modified polyetherimide comprises the following steps: Step 1) Clean the PEI sample with ethanol or acetone to remove surface impurities and oil stains, and then dry it at 60-80° C. to ensure that there is no moisture on the surface; Step 2) dissolving an appropriate amount of silane coupling agent (such as 3-aminopropyltriethoxysilane, APTES) in anhydrous ethanol to prepare a 0.5-2% solution, stirring evenly to ensure that the silane coupling agent is completely dissolved; Step 3) immersing the dried PEI sample in a silane coupling agent solution for 30-60 minutes to ensure that the silane coupling agent reacts fully with the PEI surface, and stirring slightly during the immersion process to improve the treatment effect; Step 4) taking out the treated PEI sample, washing it with anhydrous ethanol or deionized water to remove the unreacted silane coupling agent; then drying it at 60-80° C. to ensure that there is no residual solvent on the surface; Step 5) curing the dried PEI sample at 120-150° C. for 1-2 hours to ensure that the silane coupling agent forms a stable chemical bond on the surface of PEI, thereby obtaining modified polyetherimide.

3. The highly wear-resistant rubber material for automobile charging pile charging cable according to claim 1, characterized in that: The nano filler is nano silicon dioxide or nano aluminum oxide.

4. The highly wear-resistant rubber material for automobile charging pile charging cable according to claim 1, characterized in that: The plasticizer is any one of dioctyl adipate (DOA) and dioctyl sebacate (DOS), or a combination of both.

5. The highly wear-resistant rubber material for automobile charging pile charging cable according to claim 1, characterized in that: The auxiliary cross-linking agent is either TAIC or TAC or a combination of both.

6. The highly wear-resistant rubber material for automobile charging pile charging cable according to claim 1, characterized in that: The vulcanizing agent is any one of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and bis-(tert-butylperoxyisopropyl)benzene, or a combination of both.

7. A method for preparing a highly wear-resistant rubber compound for a charging cable of a vehicle charging pile according to any one of claims 1 to 6, characterized in that: The steps include: 1) All raw materials are accurately weighed by weight, and hydrogenated nitrile rubber (HNBR) and modified polyetherimide (PEI) are preliminarily mixed at room temperature to ensure that the two are evenly distributed; 2) Add the pre-mixed HNBR and PEI mixture into a twin-screw mixer, and gradually add nanofiller, plasticizer, co-crosslinking agent and vulcanizing agent; set the mixer temperature to 150-180°C and the speed to 100-200rpm; maintain uniform mixing during the mixing process to ensure that all components are fully dispersed; 3) Dynamic vulcanization is performed in the rear section of the twin-screw mixer, the vulcanization temperature is set to 180-200°C, and the vulcanization time is 5-10 minutes; 4) The mixture extruded from the twin-screw mixer is rapidly cooled by a cooling device to obtain the desired rubber compound.