Novel geomembrane as well as preparation method and application thereof

By using modified polyethylene and other materials in geomembrane, combined with specific preparation methods, the problems of easy damage during geomembrane construction and aging after use are solved, and high-performance anti-seepage and anti-ultraviolet effects are achieved, which extends the Lifespan and reduce environmental impact.

CN119060432APending Publication Date: 2024-12-03SHANDONG JIANTONG PLASTIC TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411185524.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Geofilm is prone to damage during construction, is slow to construct, and is prone to ultraviolet aging and deformation after use, resulting in a reduction in protective effect and increasing construction costs.

Method used

Modified high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-octene copolymer, anti-ultraviolet aging agent, maleic anhydride grafted ethylene propylene terephthalate, polybutyl terephthalate Materials such as glycol esters, loose fibers, polyacrylonitrile fibers and silane coupling agents improve the anti-seepage properties, mechanical strength and welding properties of geomembranes through specific preparation methods, and enhance their flexibility and UV resistance.

Benefits of technology

It achieves good anti-seepage, mechanical strength and weldability of geomembrane, extends service life, improves tensile and tear resistance, ensures stability of physical and chemical properties, and reduces environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013381900000071
    Figure BDA0005013381900000071
  • Figure BDA0005013381900000081
    Figure BDA0005013381900000081
Patent Text Reader

Abstract

The invention discloses a novel geomembrane and a preparation method and application thereof, and belongs to the technical field of geomembranes. The novel geomembrane is prepared from the following raw materials in parts by weight: 25 to 40 parts of modified high-density polyethylene, 20 to 30 parts of low-density polyethylene, 17 to 25 parts of linear low-density polyethylene, 12 to 20 parts of polyethylene, 10 to 15 parts of ethylene-octylene copolymer, 3 to 8 parts of anti-ultraviolet aging agent, 13 to 18 parts of maleic anhydride grafted ethylene propylene diene monomer, 5 to 10 parts of polybutylene terephthalate and 2 to 5 parts of loose fiber. 2-5 parts of polyacrylonitrile fiber, 1-3 parts of a silane coupling agent and 0.5-2 parts of an antioxidant. According to the present invention, the material has characteristics of simple structure, easy construction, difficult damage, good plastic deformation capacity, and excellent protection effect even if the material encounters the emergency situation or is used for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a novel geomembrane and a preparation method and application thereof, belonging to the technical field of geomembranes. Background Art

[0002] In the construction of water conservancy projects, geomembranes can protect the engineering structures from corrosion, wear and scouring. They are usually made of high-strength, corrosion-resistant polymer materials and cover the surface of the hydraulic structure to form a protective layer. Geomembrane is a polymer material with good impermeability and durability. It can effectively prevent water from damaging the structure and extend the service life of the hydraulic structure.

[0003] Since reservoirs are usually built in valleys or low-lying areas with complex geological conditions, anti-seepage measures must be taken to avoid leakage between the bottom of the reservoir and the surrounding rocks. During the construction process of geomembrane anti-seepage technology, problems such as geomembrane damage, slow construction, and how to ensure the quality of laying will occur; in addition, after a period of use, the geomembrane will undergo UV aging and deformation. At this time, once the covered surface settles or sinks, it will cause large-scale tearing of the geomembrane, which not only affects the protection effect, but also increases the construction cost. Summary of the invention

[0004] In order to solve the above problems, a new geomembrane and its preparation method and application are provided, which are conducive to construction, not easy to be damaged, and have good plastic deformation ability, and still have excellent protective effect even in the event of emergencies or after long-term use.

[0005] The technical solution adopted by the present invention is:

[0006] According to one aspect of the present application, a new geomembrane is provided, comprising the following raw materials in parts by weight: 25-40 parts of modified high-density polyethylene, 20-30 parts of low-density polyethylene, 17-25 parts of linear low-density polyethylene, 12-20 parts of polyethylene, 10-15 parts of ethylene-octene copolymer, 3-8 parts of anti-ultraviolet aging agent, 13-18 parts of maleic anhydride grafted ethylene propylene rubber, 5-10 parts of polybutylene terephthalate, 2-5 parts of pine fiber, 2-5 parts of polyacrylonitrile fiber, 1-3 parts of silane coupling agent, and 0.5-2 parts of antioxidant.

[0007] Optionally, the following raw materials are included in parts by weight: 33 parts of modified high-density polyethylene, 25 parts of low-density polyethylene, 20 parts of linear low-density polyethylene, 16 parts of polyethylene, 13 parts of ethylene-octene copolymer, 6 parts of anti-ultraviolet aging agent, 15 parts of maleic anhydride grafted ethylene propylene rubber, 8 parts of polybutylene terephthalate, 4 parts of pine fiber, 3 parts of polyacrylonitrile fiber, 2 parts of silane coupling agent, and 1 part of antioxidant.

[0008] Optionally, the method for preparing the modified high-density polyethylene comprises the following steps:

[0009] (1) titanate and isopropanol are mixed uniformly to obtain a diluted solution, and then the composite powder is dried at 90-110° C., and then the dried composite powder is added to a high-speed mixer, and the temperature is raised to 70-90° C., and the diluted solution is added to the high-speed mixer at a rate of 1-3 drops / second. After stirring uniformly, the composite powder is activated and reacted at 70-90° C. for 1-3 hours to obtain a pretreated composite powder;

[0010] (2) Add the pretreated composite powder and high-density polyethylene in a weight ratio of (0.4-0.6):1 into a high-speed mixer, stir and mix at room temperature for 5-10 minutes, and then extrude the mixture into granules through a twin-screw extruder at an extrusion temperature of 190-220° C. to obtain modified high-density polyethylene.

[0011] Optionally, the composite powder is aluminum nitride, calcite and silicon carbide in a weight ratio of (2-5):(1-3):(0.5-2).

[0012] Optionally, the titanate is used in an amount of 0.5-1 wt %.

[0013] Optionally, the anti-ultraviolet aging agent is polybenzimidazole and modified carbon black in a weight ratio of 1:(1-3).

[0014] Optionally, the silane coupling agent is selected from at least one of KH550, KH560, and KH570.

[0015] Optionally, the antioxidant is selected from at least one of tert-butyl-4-hydroxyanisole, 3,4,5-trihydroxybenzoic acid propyl ester and tert-butyl hydroquinone.

[0016] According to another aspect of the present application, there is provided a method for preparing any of the novel geomembranes described above, comprising the following steps:

[0017] S1. Place an anti-ultraviolet aging agent, maleic anhydride grafted EPDM rubber, polybutylene terephthalate, pine fiber, polyacrylonitrile fiber, silane coupling agent, and antioxidant into an internal mixer, blend and internally mix at 80-100° C. for 15-30 minutes, and extrude to obtain premixed particles;

[0018] S2, placing modified high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polyethylene, ethylene-octene copolymer and the premixed particles in step S1 into a twin-screw extruder, extruding through a die at 170-180° C. and calendering to obtain a new geomembrane.

[0019] According to another aspect of the present application, there is provided a use of any of the above-mentioned novel geomembranes for preventing leakage and anti-sedimentation in the fields of reservoirs, tailings ponds and building structural surfaces.

[0020] In this application, "normal temperature" refers to 20-30°C.

[0021] The beneficial effects of this application include but are not limited to:

[0022] 1. The new geomembrane of the present application has good anti-seepage performance, mechanical strength and weldability; wherein, the addition of modified high-density polyethylene, low-density polyethylene and linear low-density polyethylene, while ensuring that the geomembrane has excellent anti-seepage performance, also enhances its flexibility, thus being conducive to maintaining a stable anti-seepage effect in different terrains; treating the composite powder with titanate can not only improve the mixing of the composite powder and high-density polyethylene, but also establish an effective thermal conductive network structure between the two, enhance thermal conductivity, improve the weldability of the geomembrane, and at the same time improve its tensile strength and elongation at break; the composite powder used in the present application can better participate in the establishment of the thermal conductive network structure, thereby helping to better improve the thermal conductivity of the geomembrane and improve its weldability.

[0023] 2. The new geomembrane of the present application also contains an anti-ultraviolet aging agent and an antioxidant, among which polybenzimidazole and modified carbon black work synergistically to play a UV shielding role, converting the absorbed light energy into heat energy, thereby inhibiting the photo-oxidative aging degradation of the geomembrane and effectively increasing its service life; this is because polybenzimidazole can inhibit the migration of modified carbon black in the geomembrane, avoiding the agglomeration of modified carbon black particles during use, thereby effectively resisting UV aging; the addition of antioxidants can prevent the geomembrane from being degraded due to oxidation during processing and use, ensuring the stability of its physical and chemical properties.

[0024] 3. In the novel geomembrane of the present application, by adding polyethylene, ethylene-octene copolymer, maleic anhydride grafted ethylene propylene rubber and polybutylene terephthalate, good mechanical strength is provided, and the compatibility between the components is enhanced, thereby improving the tensile and tear resistance of the geomembrane; by adding loose fiber and polyacrylonitrile fiber, it not only helps to improve the mechanical properties of the geomembrane, but also improves its biodegradability and reduces the potential impact on the environment; the addition of silane coupling agent further enhances the compatibility and bonding force between the components, thereby helping to improve the overall performance of the geomembrane. DETAILED DESCRIPTION

[0025] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0026] If no specific conditions are specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials or instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.

[0027] Example 1

[0028] A method for preparing a novel geomembrane comprises the following steps:

[0029] S1. By weight, 3 parts of anti-ultraviolet aging agent (polybenzimidazole and modified carbon black in a weight ratio of 1:1), 13 parts of maleic anhydride grafted ethylene propylene rubber, 5 parts of polybutylene terephthalate, 2 parts of pine fiber, 2 parts of polyacrylonitrile fiber, 1 part of silane coupling agent KH550, and 0.5 parts of tert-butyl-4-hydroxyanisole are placed in an internal mixer, blended and internally kneaded at 80° C. for 30 minutes, and extruded to obtain premixed particles;

[0030] S2, placing 25 parts of modified high-density polyethylene, 20 parts of low-density polyethylene, 17 parts of linear low-density polyethylene, 12 parts of polyethylene, 10 parts of ethylene-octene copolymer and the premixed particles in step S1 into a twin-screw extruder, extruding through a die at 170° C. and calendering to obtain a novel geomembrane;

[0031] The method for preparing the modified high-density polyethylene comprises the following steps:

[0032] (1) 0.5 wt% titanate and isopropanol are mixed uniformly to obtain a diluted solution, and then aluminum nitride, calcium silicate, and silicon carbide are dried at a weight ratio of 2:1:0.5 at 90° C., and then the dried composite powder is added to a high-speed mixer, and the temperature is raised to 70° C., and the diluted solution is added to the high-speed mixer at a rate of 1 drop / second. After stirring uniformly, the composite powder is activated and reacted at 70° C. for 3 hours to obtain a pretreated composite powder;

[0033] (2) The pretreated composite powder and high-density polyethylene in a weight ratio of 0.4:1 were added to a high-speed mixer, stirred and mixed at room temperature for 5 minutes, and then the mixture was extruded and granulated through a twin-screw extruder at an extrusion temperature of 190° C. to obtain modified high-density polyethylene.

[0034] Example 2

[0035] A method for preparing a novel geomembrane comprises the following steps:

[0036] S1. By weight, 6 parts of anti-ultraviolet aging agent (polybenzimidazole and modified carbon black in a weight ratio of 1:2), 15 parts of maleic anhydride grafted ethylene propylene rubber, 8 parts of polybutylene terephthalate, 4 parts of pine fiber, 3 parts of polyacrylonitrile fiber, 2 parts of silane coupling agent KH560, and 1 part of 3,4,5-trihydroxybenzoic acid propyl ester are placed in an internal mixer, blended and internally kneaded at 90° C. for 20 minutes, and premixed particles are obtained after extrusion;

[0037] S2, placing 33 parts of modified high-density polyethylene, 25 parts of low-density polyethylene, 20 parts of linear low-density polyethylene, 16 parts of polyethylene, 13 parts of ethylene-octene copolymer and the premixed particles in step S1 into a twin-screw extruder, extruding through a die at 175° C. and calendering to obtain a novel geomembrane;

[0038] The method for preparing the modified high-density polyethylene comprises the following steps:

[0039] (1) 0.8 wt% titanate and isopropanol are mixed uniformly to obtain a diluted solution, and then aluminum nitride, calcium silicate, and silicon carbide are dried at a weight ratio of 4:2:1 at 100° C., and then the dried composite powder is added to a high-speed mixer, and the temperature is raised to 80° C., and the diluted solution is added to the high-speed mixer at a rate of 2 drops / second. After stirring uniformly, the composite powder is activated and reacted at 80° C. for 2 hours to obtain a pretreated composite powder;

[0040] (2) The pretreated composite powder and high-density polyethylene in a weight ratio of 0.5:1 were added to a high-speed mixer, stirred and mixed at room temperature for 8 minutes, and then the mixture was extruded and granulated through a twin-screw extruder at an extrusion temperature of 200° C. to obtain modified high-density polyethylene.

[0041] Example 3

[0042] A method for preparing a novel geomembrane comprises the following steps:

[0043] S1. By weight, 8 parts of an anti-ultraviolet aging agent (polybenzimidazole and modified carbon black in a weight ratio of 1:3), 18 parts of maleic anhydride grafted ethylene propylene rubber, 10 parts of polybutylene terephthalate, 5 parts of pine fiber, 5 parts of polyacrylonitrile fiber, 3 parts of silane coupling agent KH570, and 2 parts of tert-butyl hydroquinone are placed in an internal mixer, blended and internally kneaded at 100° C. for 15 minutes, and extruded to obtain premixed particles;

[0044] S2, placing 40 parts of modified high-density polyethylene, 30 parts of low-density polyethylene, 25 parts of linear low-density polyethylene, 20 parts of polyethylene, 15 parts of ethylene-octene copolymer and the premixed particles in step S1 into a twin-screw extruder, extruding through a die at 180° C. and calendering to obtain a novel geomembrane;

[0045] The method for preparing the modified high-density polyethylene comprises the following steps:

[0046] (1) 1 wt% titanate and isopropanol are mixed uniformly to obtain a diluted solution, and then aluminum nitride, calcium silicate, and silicon carbide are dried at a weight ratio of 5:3:2 at 110° C., and then the dried composite powder is added to a high-speed mixer, and the temperature is raised to 90° C., and the diluted solution is added to the high-speed mixer at a rate of 3 drops / second. After stirring uniformly, the composite powder is activated and reacted at 90° C. for 1 hour to obtain a pretreated composite powder;

[0047] (2) The pretreated composite powder and high-density polyethylene in a weight ratio of 0.6:1 were added to a high-speed mixer, stirred and mixed at room temperature for 10 minutes, and then the mixture was extruded and granulated through a twin-screw extruder at an extrusion temperature of 220° C. to obtain modified high-density polyethylene.

[0048] Example 4

[0049] The difference from Example 2 is that:

[0050] The polybenzimidazole and modified carbon black in a weight ratio of 1:2 were replaced by modified carbon black.

[0051] Example 5

[0052] The difference from Example 2 is that:

[0053] Titanate was replaced by silane coupling agent KH560.

[0054] Example 6

[0055] The difference from Example 2 is that:

[0056] The weight ratio of aluminum nitride, wollastonite, and silicon carbide is 1:1:1.

[0057] Comparative Example 1

[0058] The difference from Example 2 is that:

[0059] The method for preparing the modified high-density polyethylene is not disclosed, and the modified high-density polyethylene is replaced by high-density polyethylene.

[0060] Comparative Example 2

[0061] The difference from Example 2 is that:

[0062] The preparation method of modified high-density polyethylene comprises the following steps:

[0063] 0.8wt% titanate is mixed evenly with isopropanol to obtain a diluted solution, and then aluminum nitride, calcium silicate and silicon carbide in a weight ratio of 4:2:1 are dried at 100°C, and then the dried composite powder and high-density polyethylene (weight ratio of 0.5:1) are added to a high-speed mixer, and the temperature is raised to 80°C, and the diluted solution is added to the high-speed mixer at a rate of 2 drops / second. After stirring evenly, the mixture is extruded and granulated through a twin-screw extruder at an extrusion temperature of 200°C to obtain modified high-density polyethylene.

[0064] Comparative Example 3

[0065] The material of geomembrane is high-density polyethylene.

[0066] The new geomembranes prepared in Examples 1-6 and Comparative Examples 1-3 were subjected to performance tests. The tensile strength at break and the elongation at break of different samples were tested according to CJ / T234-2006 6.6, the tear strength of different samples was tested according to CJ / T234-2006 6.7, the puncture strength of different samples was tested according to CJ / T 234-2006 6.8, the UV resistance of different samples was tested according to CJ / T 234-2006 6.14, the retention of OIT at normal pressure after 1600h of ultraviolet irradiation, and the anti-seepage performance of different samples was tested according to CJ / T 234-2006 6.16. The results are shown in Table 1.

[0067] Table 1

[0068]

[0069]

[0070] It can be seen from the results in Table 1 that the new geomembrane of the present application has good mechanical strength and anti-seepage performance, and is resistant to ultraviolet radiation, ensuring the stability of its physical and chemical properties, which is beneficial to extending the service life of the geomembrane. Compared with traditional high-density polyethylene geomembranes, it has obvious advantages, has a greater market competitive advantage, and is worthy of promotion and application.

[0071] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A new type of geomembrane, characterized in that: The invention comprises the following raw materials in parts by weight: 25-40 parts of modified high-density polyethylene, 20-30 parts of low-density polyethylene, 17-25 parts of linear low-density polyethylene, 12-20 parts of polyethylene, 10-15 parts of ethylene-octene copolymer, 3-8 parts of anti-ultraviolet aging agent, 13-18 parts of maleic anhydride grafted ethylene propylene rubber, 5-10 parts of polybutylene terephthalate, 2-5 parts of pine fiber, 2-5 parts of polyacrylonitrile fiber, 1-3 parts of silane coupling agent and 0.5-2 parts of antioxidant.

2. The novel geomembrane according to claim 1 is characterized in that: The invention comprises the following raw materials in parts by weight: 33 parts of modified high-density polyethylene, 25 parts of low-density polyethylene, 20 parts of linear low-density polyethylene, 16 parts of polyethylene, 13 parts of ethylene-octene copolymer, 6 parts of anti-ultraviolet aging agent, 15 parts of maleic anhydride grafted ethylene propylene rubber, 8 parts of polybutylene terephthalate, 4 parts of pine fiber, 3 parts of polyacrylonitrile fiber, 2 parts of silane coupling agent and 1 part of antioxidant.

3. The novel geomembrane according to claim 1 is characterized in that: The preparation method of the modified high-density polyethylene comprises the following steps: (1) titanate and isopropanol are mixed uniformly to obtain a diluted solution, and then the composite powder is dried at 90-110° C., and then the dried composite powder is added to a high-speed mixer, and the temperature is raised to 70-90° C., and the diluted solution is added to the high-speed mixer at a rate of 1-3 drops / second. After stirring uniformly, the composite powder is activated and reacted at 70-90° C. for 1-3 hours to obtain a pretreated composite powder; (2) Add the pretreated composite powder and high-density polyethylene in a weight ratio of (0.4-0.6):1 into a high-speed mixer, stir and mix at room temperature for 5-10 minutes, and then extrude the mixture into granules through a twin-screw extruder at an extrusion temperature of 190-220° C. to obtain modified high-density polyethylene.

4. The novel geomembrane according to claim 3 is characterized in that: The composite powder is aluminum nitride, wollastonite and silicon carbide in a weight ratio of (2-5):(1-3):(0.5-2).

5. The novel geomembrane according to claim 3 is characterized in that: The titanate is used in an amount of 0.5-1 wt %.

6. The novel geomembrane according to claim 1 is characterized in that: The anti-ultraviolet aging agent is polybenzimidazole and modified carbon black in a weight ratio of 1:(1-3).

7. The novel geomembrane according to claim 1 is characterized in that: The silane coupling agent is selected from at least one of KH550, KH560 and KH570.

8. The novel geomembrane according to claim 1 is characterized in that: The antioxidant is selected from at least one of tert-butyl-4-hydroxyanisole, 3,4,5-trihydroxybenzoic acid propyl ester and tert-butyl hydroquinone.

9. A method for preparing the novel geomembrane according to any one of claims 1 to 8, comprising the following steps: S1. Place an anti-ultraviolet aging agent, maleic anhydride grafted EPDM rubber, polybutylene terephthalate, pine fiber, polyacrylonitrile fiber, silane coupling agent, and antioxidant into an internal mixer, blend and internally mix at 80-100° C. for 15-30 minutes, and extrude to obtain premixed particles; S2, placing modified high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polyethylene, ethylene-octene copolymer and the premixed particles in step S1 into a twin-screw extruder, extruding through a die at 170-180° C. and calendering to obtain a new geomembrane.

10. Use of the novel geomembrane according to any one of claims 1 to 8 in preventing leakage and settling in reservoirs, tailings ponds and building structural surfaces.

Citation Information

Patent Citations

  • Polyethylene resin composition used as geomembrane special material and preparation method thereof

    CN103788446A