By using modified graphene oxide and modified mesoporous silica in the cable sheath layer, the problem of thick smoke and reduced mechanical properties of the cable during combustion is solved, and excellent flame retardant and aging resistance are achieved, and the extension is achieved. The service life of the cable.
Patent Information
- Application Number
- CN202411407522.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The existing cable sheath layer materials generate a large amount of thick smoke and harmful gases during combustion, and the mechanical properties are easily reduced under the action of thermal aging, making it difficult to meet the requirements of flame retardant and aging resistance.
Modified graphene oxide and modified mesoporous silica were used as components of the sheath layer material, and prepared by chemical reactions and soft template methods to form a cable material with excellent mechanical, flame retardant and aging resistance.
The long-term flame retardant effect of cable materials is achieved, the mechanical properties and aging resistance are improved, the migration and exudation of small molecule flame retardants are avoided, and the stability and service life of the material are enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cables, and in particular relates to a reinforced halogen-free flame-retardant cable and a preparation method thereof. Background Art
[0002] With the rapid development of the economy and society, the application and demand of the cable industry in various fields are increasing. Cable materials are an important part of cables. Cable materials containing halogen flame retardants will produce a lot of smoke and harmful gases when burning, which will increase the risk of fire rescue. Therefore, halogen-free, low-smoke and flame-retardant cables have become an important direction for material preparation. The sheath layer is the first barrier of the cable. The material used to make the sheath layer should have good heat resistance and flame retardancy to play a protective role.
[0003] The traditional cable sheath layer uses polyolefins. Although it has high electrical strength, it has poor flame retardancy and aging resistance. In order to improve the flame retardancy of cable materials, the existing technology often adds a large amount of inorganic flame retardants. The currently commonly used small molecule flame retardants mainly include: halogen-containing flame retardants, phosphorus flame retardants, silicon flame retardants, nitrogen flame retardants and composite flame retardants. Due to the poor compatibility of small molecule flame retardants with materials, the mechanical properties of the materials will be reduced, and the viscosity, compatibility and flexibility of the polymer materials will also be deteriorated. In addition, the existing technology introduces non-reactive cyclotriphosphazene derivatives into the sheath layer material by physical blending, which has the problem of migration and seepage, and the stability of the performance of the obtained product is generally poor; and in the actual application process, the cable material must withstand thermal aging, and its mechanical properties are facing serious aging threats. The conventional practice is to add antioxidants, but antioxidants are easy to migrate in the base material, causing the base material's aging resistance to decrease, and other properties such as corrosion resistance and mechanical strength will be affected by aging and reduced, affecting the service life of the cable. Summary of the invention
[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a reinforced halogen-free flame retardant cable and a preparation method, which gives the cable excellent mechanical properties, flame retardant properties and aging resistance by adding modified graphene oxide and modified mesoporous silica.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A reinforced halogen-free flame-retardant cable comprises a conductor core, an insulating layer, a shielding layer and a sheath layer which are sequentially arranged from the inside to the outside. The sheath layer is prepared by pulling a sheath layer material out of the outer periphery of the shielding layer through an extrusion device. The sheath layer material comprises the following components in parts by weight: 60-70 parts of low-density polyethylene, 20-35 parts of ethylene-vinyl acetate copolymer, 5-10 parts of modified graphene oxide, 2-5 parts of modified mesoporous silica, 1-3 parts of lubricant, 1-2 parts of plasticizer and 0.1-0.5 parts of light stabilizer. The modified graphene oxide is prepared by grafting a hexachlorocyclotriphosphazene derivative with graphene oxide through a chemical reaction, wherein the hexachlorocyclotriphosphazene derivative is prepared by using 2-allylphenol, sodium hydroxide, hexachlorocyclotriphosphazene, 4,4'-diaminodiphenylmethane and DOPO as raw materials; the modified mesoporous silica is prepared by using mesoporous silica as a carrier to load iron oxide particles, and further using 3-mercaptopropylmethyldimethoxysilane to graft an antioxidant N-(4-anilinophenyl)maleimide.
[0006] Preferably, the method for preparing the sheath layer material comprises the following steps: uniformly mixing parts by weight of low-density polyethylene, ethylene-vinyl acetate copolymer, modified graphene oxide, modified mesoporous silica, lubricant, plasticizer and light stabilizer to obtain a mixture, placing the mixture into a twin-screw extruder for extrusion molding to prepare the sheath layer material.
[0007] Preferably, the method for preparing the modified graphene oxide comprises the following steps: (1) 2-allylphenol and sodium hydroxide are placed in a reactor, reacted for 25-40 minutes under nitrogen protection, then heated to 60-75°C for 0.5-1 hour, and then hexachlorocyclotriphosphazene is added to continue the reaction for 18-24 hours. After the reaction is completed, the flame retardant intermediate is prepared by rotary evaporation and drying; (2) Put the flame retardant intermediate in a reactor, add acetonitrile to dissolve it, raise the temperature to 40-55°C, add 4,4'-diaminodiphenylmethane and triethylamine to reflux for 6-8h to prepare component A, dissolve DOPO in acetonitrile and add it to component A, and react at 75-90°C for 5-7h. After the reaction is completed, filter, wash and dry to prepare a hexachlorocyclotriphosphazene derivative; (3) Ultrasonic dispersion of graphene oxide in ethanol is performed to obtain a graphene oxide dispersion. Deionized water, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are mixed evenly and added to the graphene oxide dispersion. Then, a hexachlorocyclotriphosphazene derivative is added and stirred at 40-55°C for 4-7 hours. After the reaction is completed, the modified graphene oxide is prepared by centrifugation, washing and drying.
[0008] Preferably, in the step (1), the molar ratio of 2-allylphenol, sodium hydroxide and hexachlorocyclotriphosphazene is 1-1.04:1-1.05:0.27-0.33; and in the step (2), the molar ratio of the flame retardant intermediate, 4,4'-diaminodiphenylmethane and DOPO is 1:3-3.3:3-3.5.
[0009] Preferably, the method for preparing the modified mesoporous silica comprises the following steps: A. Take hexadecyltrimethylammonium bromide and sodium hydroxide in a reactor, add deionized water, dissolve with ultrasonic vibration, place at 75-85°C and stir for 10-20 minutes, then add tetraethyl orthosilicate and continue stirring for 2-3 hours. After the reaction is completed, centrifuge, wash and dry, ultrasonically disperse the obtained solid product in a mixed solution of methanol and hydrochloric acid, place under cooling reflux conditions at 50-65°C, stir vigorously for 42-48 hours to remove the surfactant, centrifuge, wash and dry to prepare mesoporous silica; B. Dissolve ferric chloride nonahydrate in ethanol to obtain a mixed solution, add mesoporous silica to disperse evenly by ultrasonication, stir at 85-95°C until dry, and then calcine at 150-200°C for 1.5-2h, add the obtained product to the mixed solution of ferric chloride nonahydrate and ethanol again, stir at 85-95°C until dry, and then calcine at 350-400°C for 3-4h to prepare functionalized mesoporous silica; C. Take N-(4-anilinophenyl)maleimide and 3-mercaptopropylmethyldimethoxysilane and dissolve them in acetone. Heat the temperature to 40-50°C under nitrogen protection, add triethylamine and stir to react for 4-5 hours to obtain component one. Take functionalized mesoporous silica and ultrasonically disperse it in a mixed solution of ethanol and deionized water, add ammonia water to adjust the pH value of the mixed solution to 9-10, heat the temperature to 55-65°C, add component one and stir to react for 4-6 hours. After the reaction is completed, centrifuge, wash and dry to prepare modified mesoporous silica.
[0010] Preferably, in step A, the molar ratio of hexadecyltrimethylammonium bromide, sodium hydroxide and tetraethyl orthosilicate is 1-1.2:2.2-2.8:8.1-9.6.
[0011] Preferably, in step C, the mass ratio of N-(4-anilinophenyl)maleimide, 3-mercaptopropylmethyldimethoxysilane and functionalized mesoporous silica is 0.4-1:0.3-0.9:5-10 g.
[0012] Preferably, the lubricant is polyethylene wax or oxidized polyethylene wax; the plasticizer is one or more combinations of dioctyl adipate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate; and the light stabilizer is one or more combinations of light stabilizer 770, light stabilizer 944, and light stabilizer 2020.
[0013] Preferably, the insulating layer uses cross-linked polyethylene or polyethylene as the insulating material; the shielding layer includes a first shielding layer and a second shielding layer, the first shielding layer is made of aluminum foil wrapping, and the second shielding layer is made of silver-plated copper wire weaving.
[0014] The method for preparing the reinforced halogen-free flame-retardant cable as described above comprises the following steps: S1. Using a wire drawing machine to draw the copper rod to obtain a copper wire, and then annealing the wire to obtain a conductor; S2, twisting at least two of the conductors together to obtain a conductor core; S3, using an extruder to extrude an insulating layer on the outer surface of the conductor core; S4, wrap aluminum foil around the outer surface of the insulation layer to obtain a first shielding layer, and cross-weave silver-plated copper wire on the outer surface of the first shielding layer to obtain a second shielding layer; S5. Extruding a sheath layer on the outer surface of the second shielding layer to prepare a reinforced halogen-free flame-retardant cable.
[0015] Beneficial effects of the present invention: The invention uses 2-allylphenol and sodium hydroxide as raw materials to replace three chlorine atoms in a hexachlorocyclotriphosphazene structure, thereby preparing a flame retardant intermediate with a double bond group introduced into the structure; then the flame retardant intermediate is reacted with 4,4'-diaminodiphenylmethane, so that the remaining three chlorine atoms in the structure of the flame retardant intermediate undergo a substitution reaction with an amino group at one end of the 4,4'-diaminodiphenylmethane structure, thereby introducing an amino group into the structure of the flame retardant intermediate, thereby preparing a component A with a double bond group and an amino group introduced into the structure; then the component A is further grafted with DOPO, so that the double bond group in the structure of the component A undergoes an addition reaction with a PH bond in the structure of DOPO, thereby preparing a hexachlorocyclotriphosphazene derivative rich in phosphorus and nitrogen elements, forming a nitrogen-phosphorus synergistic flame retardant effect, and achieving excellent flame retardant effect and heat resistance; finally, the obtained hexachlorocyclotriphosphazene derivative undergoes an amidation reaction with graphene oxide, thereby preparing modified graphene oxide. Among them, graphene oxide has excellent mechanical properties. The hexachlorocyclotriphosphazene derivatives are introduced into the graphene oxide layered structure, giving the material excellent flame retardant properties. At the same time, the two are combined through a strong chemical bond to avoid the problem of migration and seepage of hexachlorocyclotriphosphazene derivatives, ensuring that the material achieves long-term flame retardant effect. In addition, the grafting reaction increases the interlayer spacing of graphene oxide, which is beneficial to the dispersion of graphene oxide and avoids the performance defects caused by graphene oxide agglomeration to a certain extent.
[0016] The present invention uses a soft template method to prepare mesoporous silica, and uses mesoporous silica as a carrier to load iron oxide to prepare functionalized mesoporous silica, wherein the mesoporous structure of the mesoporous silica can absorb and catalyze the combustible gas generated by the material into carbon, and the loaded iron oxide particles have more active sites, and the material has a stronger catalytic carbonization ability when it burns, and at the same time, it has a stronger absorption ability for the combustible gas generated by the combustion of the material, and it is added to the matrix as a synergist to further improve the flame retardancy and mechanical properties of the cable material. At the same time, the present invention uses 3-mercaptopropylmethyldimethoxysilane to graft the antioxidant N-(4-anilinophenyl)maleimide on the surface of the functionalized mesoporous silica to prepare modified mesoporous silica, and N-(4-anilinophenyl)maleimide and the functionalized mesoporous silica are firmly combined through chemical bonds, giving the cable material excellent aging resistance, and at the same time avoiding the problem of easy volatilization, migration and extraction of the antioxidant during processing or long-term use. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1 A method for preparing modified graphene oxide comprises the following steps: (1) 13.9 g of 2-allylphenol and 4.15 g of sodium hydroxide were placed in a reactor, reacted for 30 min under nitrogen protection, then heated to 70 °C for 1 h, then 10 g of hexachlorocyclotriphosphazene was added and the reaction continued for 24 h. After the reaction was completed, the mixture was subjected to rotary evaporation and drying to obtain a flame retardant intermediate; (2) 6.41 g of the flame retardant intermediate was placed in a reactor, 200 mL of acetonitrile was added to dissolve it, the temperature was raised to 50°C, 5.97 g of 4,4'-diaminodiphenylmethane and 3 g of triethylamine were added to reflux for 8 h to prepare component A, 6.52 g of DOPO was dissolved in 40 mL of acetonitrile and added to component A, and the mixture was reacted at 85°C for 7 h. After the reaction was completed, the mixture was filtered, washed and dried to prepare a hexachlorocyclotriphosphazene derivative; (3) 5 g of graphene oxide was ultrasonically dispersed in 120 mL of ethanol to obtain a graphene oxide dispersion. 30 mL of deionized water, 0.02 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.03 g of N-hydroxysuccinimide were mixed evenly and added to the graphene oxide dispersion. Then, 0.8 g of a hexachlorocyclotriphosphazene derivative was added. The mixture was stirred at 40-55 °C for 4-7 h. After the reaction was completed, the modified graphene oxide was prepared by centrifugation, washing and drying.
[0019] Example 2 A method for preparing modified mesoporous silica comprises the following steps: A. Take 1g of hexadecyltrimethylammonium bromide and 0.28g of sodium hydroxide in a reactor, add 450mL of deionized water, ultrasonically shake to dissolve, place at 80°C and stir for 15min, then add 5.92g of tetraethyl orthosilicate and continue stirring to react for 2h. After the reaction is completed, centrifuge, wash and dry, ultrasonically disperse the obtained solid product in a mixed solution of methanol and hydrochloric acid, place under cooling reflux at 60°C, vigorously stir for 48h to remove the surfactant, centrifuge, wash and dry to prepare mesoporous silica; B. Take 6 mmol of ferric chloride nonahydrate and dissolve it in 100 mL of ethanol to obtain a mixed solution, add 4.3 g of mesoporous silica and disperse it evenly by ultrasonication, stir it at 95°C until it is dry, and then calcine it at 195°C for 2 hours. The obtained product is added again to a mixed solution of 6 mmol of ferric chloride nonahydrate and 100 mL of ethanol, stir it at 95°C until it is dry, and then calcine it at 400°C for 3.5 hours to prepare functionalized mesoporous silica; C. Take 0.86g of N-(4-anilinophenyl)maleimide and 0.64g of 3-mercaptopropylmethyldimethoxysilane and dissolve them in 50mL of acetone. Heat to 45°C under nitrogen protection, add 0.4g of triethylamine and stir to react for 5h to obtain component one. Take 5g of functionalized mesoporous silica and ultrasonically disperse it in a mixed solution of 90mL of ethanol and 20mL of deionized water. Add ammonia water to adjust the pH value of the mixed solution to 10, heat to 60°C, add component one and stir to react for 5h. After the reaction is completed, centrifuge, wash and dry to prepare modified mesoporous silica.
[0020] Example 3 A sheath layer material includes the following components in parts by weight: 60 parts of low-density polyethylene, 21 parts of ethylene-vinyl acetate copolymer, 5 parts of modified graphene oxide prepared in Example 1, 2 parts of modified mesoporous silica prepared in Example 2, 1 part of lubricant polyethylene wax, 1 part of plasticizer dioctyl adipate, 0.2 parts of light stabilizer 2020; The preparation method of the above-mentioned sheath layer material comprises the following steps: uniformly mixing weight parts of low-density polyethylene, ethylene-vinyl acetate copolymer, modified graphene oxide, modified mesoporous silica, lubricant, plasticizer and light stabilizer to obtain a mixture, placing the mixture into a twin-screw extruder for extrusion molding, and preparing the sheath layer material.
[0021] A reinforced halogen-free flame-retardant cable comprises a conductor core, an insulating layer, a shielding layer, and a sheath layer arranged in sequence from the inside to the outside, and a preparation method thereof comprises the following steps: S1. Using a wire drawing machine to draw the copper rod to obtain a copper wire, and then annealing the wire to obtain a conductor; S2, twisting at least two of the conductors together to obtain a conductor core; S3, using an extruder to extrude an insulating layer on the outer surface of the conductor core; S4, wrap aluminum foil around the outer surface of the insulation layer to obtain a first shielding layer, and cross-weave silver-plated copper wire on the outer surface of the first shielding layer to obtain a second shielding layer; S5. Extruding a sheath layer on the outer surface of the second shielding layer to prepare a reinforced halogen-free flame-retardant cable.
[0022] Example 4 A sheath layer material includes the following components in parts by weight: 65 parts of low-density polyethylene, 27 parts of ethylene-vinyl acetate copolymer, 7 parts of modified graphene oxide prepared in Example 1, 4 parts of modified mesoporous silica prepared in Example 2, 2 parts of lubricant oxidized polyethylene wax, 2 parts of plasticizer dimethyl phthalate, 0.3 parts of light stabilizer 944; The preparation method of the above-mentioned sheath layer material and the preparation method of the reinforced halogen-free flame-retardant cable are the same as those in Example 3.
[0023] Example 5 A sheath layer material includes the following components in parts by weight: 70 parts of low-density polyethylene, 34 parts of ethylene-vinyl acetate copolymer, 10 parts of modified graphene oxide prepared in Example 1, 5 parts of modified mesoporous silica prepared in Example 2, 3 parts of lubricant polyethylene wax, 2 parts of plasticizer dioctyl phthalate, 0.5 parts of light stabilizer 770; The preparation method of the above-mentioned sheath layer material and the preparation method of the reinforced halogen-free flame-retardant cable are the same as those in Example 3.
[0024] Comparative Example 1 A method for preparing modified mesoporous silica comprises the following steps: A. Take 1g of hexadecyltrimethylammonium bromide and 0.28g of sodium hydroxide in a reactor, add 450mL of deionized water, ultrasonically shake to dissolve, place at 80°C and stir for 15min, then add 5.92g of tetraethyl orthosilicate and continue stirring to react for 2h. After the reaction is completed, centrifuge, wash and dry, ultrasonically disperse the obtained solid product in a mixed solution of methanol and hydrochloric acid, place under cooling reflux at 60°C, vigorously stir for 48h to remove the surfactant, centrifuge, wash and dry to prepare mesoporous silica; B. Take 0.86g of N-(4-anilinophenyl)maleimide and 0.64g of 3-mercaptopropylmethyldimethoxysilane and dissolve them in 50mL of acetone. Heat to 45°C under nitrogen protection, add 0.4g of triethylamine and stir to react for 5h to obtain component one. Take 5g of mesoporous silica and ultrasonically disperse it in a mixed solution of 90mL of ethanol and 20mL of deionized water, add ammonia water to adjust the pH value of the mixed solution to 10, heat to 60°C, add component one and stir to react for 5h. After the reaction is completed, centrifuge, wash and dry to prepare modified mesoporous silica.
[0025] Comparative Example 2 A method for preparing modified mesoporous silica comprises the following steps: A. Take 1g of hexadecyltrimethylammonium bromide and 0.28g of sodium hydroxide in a reactor, add 450mL of deionized water, ultrasonically shake to dissolve, place at 80°C and stir for 15min, then add 5.92g of tetraethyl orthosilicate and continue stirring to react for 2h. After the reaction is completed, centrifuge, wash and dry, ultrasonically disperse the obtained solid product in a mixed solution of methanol and hydrochloric acid, place under cooling reflux at 60°C, vigorously stir for 48h to remove the surfactant, centrifuge, wash and dry to prepare mesoporous silica; B. Take 6 mmol of ferric chloride nonahydrate and dissolve it in 100 mL of ethanol to obtain a mixed solution, add 4.3 g of mesoporous silica and disperse it evenly by ultrasonication, stir at 95°C until dry, and then calcine at 195°C for 2 h. The obtained product is added again to a mixed solution of 6 mmol of ferric chloride nonahydrate and 100 mL of ethanol, stir at 95°C until dry, and then calcine at 400°C for 3.5 h to prepare modified mesoporous silica.
[0026] Comparative Example 3 A sheath layer material comprises the following components in parts by weight: 70 parts of low-density polyethylene, 34 parts of ethylene-vinyl acetate copolymer, 10 parts of graphene oxide, 5 parts of modified mesoporous silica prepared in Example 2, 3 parts of lubricant polyethylene wax, 2 parts of plasticizer dioctyl phthalate, and 7700.5 parts of light stabilizer; The preparation method of the above-mentioned sheath layer material and the preparation method of the reinforced halogen-free flame-retardant cable are the same as those in Example 3.
[0027] Comparative Example 4 A sheath layer material comprises the following components in parts by weight: 70 parts of low-density polyethylene, 34 parts of ethylene-vinyl acetate copolymer, 10 parts of modified graphene oxide prepared in Example 1, 5 parts of modified mesoporous silica prepared in Comparative Example 1, 3 parts of lubricant polyethylene wax, 2 parts of plasticizer dioctyl phthalate, 0.5 parts of light stabilizer 770; The preparation method of the above-mentioned sheath layer material and the preparation method of the reinforced halogen-free flame-retardant cable are the same as those in Example 3.
[0028] Comparative Example 5 A sheath layer material comprises the following components in parts by weight: 70 parts of low-density polyethylene, 34 parts of ethylene-vinyl acetate copolymer, 10 parts of modified graphene oxide prepared in Example 1, 5 parts of modified mesoporous silica prepared in Comparative Example 2, 3 parts of lubricant polyethylene wax, 2 parts of plasticizer dioctyl phthalate, 0.5 parts of light stabilizer 770; The preparation method of the above-mentioned sheath layer material and the preparation method of the reinforced halogen-free flame-retardant cable are the same as those in Example 3.
[0029] Performance Testing The sheath layer materials prepared in Examples 3-5 and Comparative Examples 3-5 were subjected to performance testing: a tensile performance test was performed using a universal mechanical testing machine in accordance with GB / T 1040.2-2022 standard, and the change rates of tensile strength and elongation at break were tested after aging at 110°C for 48h and 72h, an impact strength test was performed in accordance with GB / T1843-2008 standard, and a tear strength test was performed in accordance with GB / T 529-2008 standard; the flame retardant properties were tested using a limiting oxygen index test and a vertical burning test, and the data results are shown in Table 1.
[0030] Table 1 Test results of sample performance
[0031] It can be seen from the data in Table 1 that the sheath layer materials prepared in Examples 3-5 of the present invention have excellent mechanical properties, flame retardant properties and aging resistance. In Comparative Example 3, graphene oxide was not modified, and the mechanical properties measured were lower than those of Examples 3-5, which may be due to the agglomeration of graphene oxide, resulting in reduced mechanical properties, and due to the lack of grafting of hexachlorocyclotriphosphazene derivatives, resulting in poorer flame retardant properties than those of Examples 3-5. The modified mesoporous silica added in Comparative Example 4 was not loaded with iron oxide, and the mechanical properties and flame retardant properties measured were slightly worse than those of Examples 3-5, indicating that the loading of iron oxide can be used as a synergist to further improve the flame retardant and mechanical properties of the material. The modified mesoporous silica added in Comparative Example 5 was not grafted with an antioxidant, resulting in poor dispersibility, and the mechanical properties measured were lower than those of Examples 3-5, and the change rate of tensile strength and elongation at break were significantly changed compared with Examples 3-5, indicating that the grafting of antioxidants can give the material excellent aging resistance.
[0032] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0033] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A reinforced halogen-free flame-retardant cable, characterized in that: The invention comprises a conductor core, an insulating layer, a shielding layer and a sheath layer which are sequentially arranged from the inside to the outside. The sheath layer is prepared by pulling out a sheath layer material from the periphery of the shielding layer through an extrusion device. The sheath layer material comprises the following components in parts by weight: 60 to 70 parts of low-density polyethylene, 20 to 35 parts of ethylene-vinyl acetate copolymer, 5 to 10 parts of modified graphene oxide, 2 to 5 parts of modified mesoporous silica, 1 to 3 parts of lubricant, 1 to 2 parts of plasticizer and 0.1 to 0.5 parts of light stabilizer. The modified graphene oxide is prepared by grafting a hexachlorocyclotriphosphazene derivative with graphene oxide through a chemical reaction, wherein the hexachlorocyclotriphosphazene derivative is prepared by using 2-allylphenol, sodium hydroxide, hexachlorocyclotriphosphazene, 4,4'-diaminodiphenylmethane and DOPO as raw materials; the modified mesoporous silica is prepared by using mesoporous silica as a carrier to load iron oxide particles, and further using 3-mercaptopropylmethyldimethoxysilane to graft an antioxidant N-(4-anilinophenyl)maleimide.
2. The reinforced halogen-free flame-retardant cable according to claim 1, characterized in that: The preparation method of the sheath layer material comprises the following steps: uniformly mixing parts by weight of low-density polyethylene, ethylene-vinyl acetate copolymer, modified graphene oxide, modified mesoporous silica, a lubricant, a plasticizer and a light stabilizer to obtain a mixture, and extruding the mixture into a twin-screw extruder to prepare the sheath layer material.
3. The reinforced halogen-free flame-retardant cable according to claim 1, characterized in that: The preparation method of the modified graphene oxide comprises the following steps: (1) 2-allylphenol and sodium hydroxide are placed in a reactor, reacted for 25-40 minutes under nitrogen protection, then heated to 60-75°C for 0.5-1 hour, and then hexachlorocyclotriphosphazene is added to continue the reaction for 18-24 hours. After the reaction is completed, the flame retardant intermediate is prepared by rotary evaporation and drying; (2) Put the flame retardant intermediate in a reactor, add acetonitrile to dissolve it, raise the temperature to 40-55°C, add 4,4'-diaminodiphenylmethane and triethylamine to reflux for 6-8h to prepare component A, dissolve DOPO in acetonitrile and add it to component A, and react at 75-90°C for 5-7h. After the reaction is completed, filter, wash and dry to prepare a hexachlorocyclotriphosphazene derivative; (3) Ultrasonic dispersion of graphene oxide in ethanol is performed to obtain a graphene oxide dispersion. Deionized water, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are mixed evenly and added to the graphene oxide dispersion. Then, a hexachlorocyclotriphosphazene derivative is added and stirred at 40-55°C for 4-7 hours. After the reaction is completed, the modified graphene oxide is prepared by centrifugation, washing and drying.
4. The reinforced halogen-free flame-retardant cable according to claim 3, characterized in that: In the step (1), the molar ratio of 2-allylphenol, sodium hydroxide and hexachlorocyclotriphosphazene is 1-1.04:1-1.05:0.27-0.33; and in the step (2), the molar ratio of the flame retardant intermediate, 4,4'-diaminodiphenylmethane and DOPO is 1:3-3.3:3-3.
5.
5. The reinforced halogen-free flame-retardant cable according to claim 1, characterized in that: The preparation method of the modified mesoporous silica comprises the following steps: A. Take hexadecyltrimethylammonium bromide and sodium hydroxide in a reactor, add deionized water, dissolve with ultrasonic vibration, place at 75-85°C and stir for 10-20 minutes, then add tetraethyl orthosilicate and continue stirring for 2-3 hours. After the reaction is completed, centrifuge, wash and dry, ultrasonically disperse the obtained solid product in a mixed solution of methanol and hydrochloric acid, place under cooling reflux conditions at 50-65°C, stir vigorously for 42-48 hours to remove the surfactant, centrifuge, wash and dry to prepare mesoporous silica; B. Dissolve ferric chloride nonahydrate in ethanol to obtain a mixed solution, add mesoporous silica to disperse evenly by ultrasonication, stir at 85-95°C until dry, and then calcine at 150-200°C for 1.5-2h, add the obtained product to the mixed solution of ferric chloride nonahydrate and ethanol again, stir at 85-95°C until dry, and then calcine at 350-400°C for 3-4h to prepare functionalized mesoporous silica; C. Take N-(4-anilinophenyl)maleimide and 3-mercaptopropylmethyldimethoxysilane and dissolve them in acetone. Heat the temperature to 40-50°C under nitrogen protection, add triethylamine and stir to react for 4-5 hours to obtain component one. Take functionalized mesoporous silica and ultrasonically disperse it in a mixed solution of ethanol and deionized water, add ammonia water to adjust the pH value of the mixed solution to 9-10, heat the temperature to 55-65°C, add component one and stir to react for 4-6 hours. After the reaction is completed, centrifuge, wash and dry to prepare modified mesoporous silica.
6. The reinforced halogen-free flame-retardant cable according to claim 5, characterized in that: In the step A, the molar ratio of hexadecyltrimethylammonium bromide, sodium hydroxide and tetraethyl orthosilicate is 1-1.2:2.2-2.8:8.1-9.
6.
7. The reinforced halogen-free flame-retardant cable according to claim 5, characterized in that: In the step C, the mass ratio of N-(4-anilinophenyl)maleimide, 3-mercaptopropylmethyldimethoxysilane and functionalized mesoporous silica is 0.4-1:0.3-0.9:5-10 g.
8. The reinforced halogen-free flame-retardant cable according to claim 1, characterized in that: The lubricant is polyethylene wax or oxidized polyethylene wax; the plasticizer is one or more combinations of dioctyl adipate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate; the light stabilizer is one or more combinations of light stabilizer 770, light stabilizer 944, and light stabilizer 2020.
9. The reinforced halogen-free flame-retardant cable according to claim 1, characterized in that: The insulating layer uses cross-linked polyethylene or polyethylene as the insulating material; the shielding layer includes a first shielding layer and a second shielding layer, the first shielding layer is made of aluminum foil wrapping, and the second shielding layer is made of silver-plated copper wire weaving.
10. A method for preparing a reinforced halogen-free flame-retardant cable according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Using a wire drawing machine to draw the copper rod to obtain a copper wire, and then annealing the wire to obtain a conductor; S2, twisting at least two of the conductors together to obtain a conductor core; S3, using an extruder to extrude an insulating layer on the outer surface of the conductor core; S4, wrap aluminum foil around the outer surface of the insulation layer to obtain a first shielding layer, and cross-weave silver-plated copper wire on the outer surface of the first shielding layer to obtain a second shielding layer; S5. Extruding a sheath layer on the outer surface of the second shielding layer to prepare a reinforced halogen-free flame-retardant cable.
Citation Information
Patent Citations
Polyolefin flame retardant
CN105199182A
Novel bio-based phosphorus-nitrogen flame retardant additive and flame retardant epoxy resin prepared from same
CN109762203A
Low-smoke halogen-free flame-retardant irradiation crosslinking cable material for energy storage cable and preparation method of low-smoke halogen-free flame-retardant irradiation crosslinking cable material
CN118620316A
Modified graphene oxide, modified graphene oxide flame-retardant synergist, halogen-free flame-retardant polyolefin cable material, preparation method of halogen-free flame-retardant polyolefin cable material and cable
CN118725406A
Halogen-free resin composition and method for preparation of copper clad laminate with same
US20140150963A1
Cited By
High-temperature-resistant low-smoke halogen-free flame-retardant twisted-pair cable for building security system and preparation method thereof
CN119274890A
Solvent-resistant antirust anticorrosive biological resin coating and preparation method thereof
CN119708955A
Weather-proof decorative waterborne polyurethane mortar color sand self-leveling floor material
CN119912221A
Self-repairing silicone rubber flame-retardant protective pad for high-temperature welding and preparation method thereof
CN119931345A
Self-healing silicone rubber flame retardant protective pad for high-temperature welding and its preparation method
CN119931345B