Coal seam manhole sealing material and preparation method thereof

Through the combination of sodium silicate-citric acid, PVA-borax double coagulation mechanism and xanthan gum, the problems of inconvenience in construction of coal seam hole-probe sealing materials and environmental pollution are solved, and efficient and safe coal seam hole-probe sealing effect is achieved.

CN119060481APending Publication Date: 2024-12-03BEIJING HANGTIAN SAIDE TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411317446.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing coal seam hole-probe sealing materials have inconveniences and defects in construction and effect, especially the problems of inconvenience of underground mixing, high cost and environmental pollution.

Method used

The dual coagulation mechanism of sodium silicate-citric acid and PVA-borax is adopted, supplemented by xanthan gum to improve toughness and retain moisture, and the coal seam probe hole is injected into the peristaltic pump to achieve rapid sealing.

Benefits of technology

It has achieved safety and environmental protection, low cost, controllable gel time, high hardness and high toughness, excellent sealing effect, reducing the risk of gas extraction in coal seam exploration and improving exploration safety and gas utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060481A_ABST
    Figure CN119060481A_ABST
Patent Text Reader

Abstract

The invention discloses a coal seam manhole sealing material and a preparation method thereof. The sealing material comprises a material A and a material B, the material A and the material B are respectively configured and stored, and are simultaneously injected into a coal seam manhole through a peristaltic pump during use to realize manhole plugging; the material A is a mixed solution of PVA, xanthan gum, sodium silicate and water; the material B is a mixed solution of borax, citric acid and water. A sodium silicate-citric acid and PVA-borax double-coagulation mechanism in the material A and the material B is utilized, xanthan gum is supplemented to improve toughness and retain moisture, sodium chloride and matting powder are used for improving strength, the materials only need to be pumped into a manhole at the same time according to a specific pump speed ratio during construction, self-gel sealing can be achieved within a certain period of time, and the construction efficiency is greatly improved. The plugging agent has the advantages of being safe, environmentally friendly, low in cost, controllable in gelation time, high in hardness and toughness, excellent in plugging effect, convenient to construct and the like, effectively solves the problem of negative-pressure gas extraction in existing coal seam exploration and mining, reduces the danger coefficient, improves exploration and mining safety and meets the requirement for later utilization of gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal seam prospecting and mining, and in particular to a coal seam exploration hole sealing material and a preparation method thereof. Background Art

[0002] Coalbed methane, also known as coalbed methane or coal mine gas, is an unconventional natural gas that is abundant in coal seams in an adsorbed state. The methane content is greater than 90%. With good environmental, economic and social benefits, it is the most realistic replacement energy for natural gas. Therefore, the exploration and development of coalbed methane has received more and more attention. However, safety and mining purity in exploration and mining have become issues that need to be urgently addressed.

[0003] Coal seam exploration requires continuous drilling to confirm the location of the coal seam. These holes are generally deep and small in diameter, and there is gas in the coal rock. As the exploration progresses, it is necessary to continuously use negative pressure fans to extract the gas in the mine, but the presence of the sampling holes will cause the water vapor and air in the rock cracks to be extracted together, which not only increases the risk level, but also reduces the gas concentration, affecting the subsequent comprehensive utilization of the gas. Therefore, all sampling holes (i.e., exploration holes) need to be sealed before extracting the gas.

[0004] At present, most of the methods used to seal the exploration holes are to use cement mixing slurry for plugging. The difficulty is that it requires mixing and construction underground, which brings many inconveniences to equipment and operations. There are also studies and applications of using organic materials such as epoxy resin for plugging. Although the effect is good, the cost is high and it pollutes the environment.

[0005] It can be seen that the above existing coal seam exploration hole sealing materials still have inconveniences and defects in construction and results, and are in urgent need of further improvement. How to create a new coal seam exploration hole sealing material and its preparation method to overcome the shortcomings of the existing sealing materials. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a coal seam exploration hole sealing material, which improves the composition of the sealing material, utilizes the double coagulation mechanism of sodium silicate-citric acid and PVA-borax, and is supplemented with xanthan gum to improve toughness and retain moisture, thereby not only improving the sealing effect and controlling the gel time, but also the raw materials are cheap and environmentally friendly, and the construction is convenient, thereby overcoming the shortcomings of existing sealing materials.

[0007] In order to solve the above technical problems, the present invention provides a coal seam exploration hole sealing material, including material A and material B. The material A and material B are configured and stored separately, and when in use, they are simultaneously injected into the coal seam exploration hole through a peristaltic pump to achieve exploration hole sealing; the material A is a mixture of PVA, xanthan gum, sodium silicate and water; the material B is a mixture of borax, citric acid and water.

[0008] Further improvement, the preparation method of the material A is:

[0009] S1: Slowly add PVA powder into warm water at 50-80℃ while stirring continuously. Keep warm at 90℃ for 1-2h to obtain a completely dispersed PVA solution. Note: The water temperature should not be too high during preparation, otherwise the PVA powder added later will cross-link itself and make it difficult to disperse.

[0010] S2: Slowly add the xanthan gum powder into warm water at 50-70°C while stirring continuously. After the addition is completed, continue stirring at 100°C for 15-30 minutes to obtain a xanthan gum solution;

[0011] S3: adding the xanthan gum solution, the PVA solution and water just prepared into the sodium silicate solution under constant stirring to obtain the material A;

[0012] Further improvement, the configuration concentration of the PVA solution in step S1 is 15-20%. If the concentration of the PVA is too high, it is not easy to dissolve, and the reaction rate is too fast when encountering borax in the later stage, which affects the gel effect. If the concentration of the PVA is too low, a high-strength cross-linked body cannot be formed, which also affects the final gel effect; the configuration concentration of the xanthan gum solution in step S2 is 10-15%, and the xanthan gum has excellent acid and alkali resistance, and plays a role of thickening and water retention in the present invention; the configuration concentration of the sodium silicate solution in step S3 is 20%-30%, and the mass ratio of the sodium silicate solution, water, PVA solution, and xanthan gum solution in step S3 is 3-4:1:4:0.5.

[0013] Further improvement, the preparation method of the material B is:

[0014] Q1: Add borax solid and glycerol into water to prepare borax solution;

[0015] Q2: Prepare citric acid solution;

[0016] Q3: Add the citric acid mixed solution to the borax solution to obtain the material B.

[0017] In a further improvement, sodium chloride and low pore volume matting powder are also added to the citric acid solution.

[0018] Further improvement, the configuration concentration of the borax solution in step Q1 is 5-10%, wherein propylene glycol is used as a solubilizer to increase the solubility of borax in water; the configuration concentration of the citric acid solution in step Q2 is 30-50%, and the mass ratio of the citric acid solution to the added sodium chloride solid and the low pore volume matting powder is 1:0.2:0.1-0.2 to form a citric acid mixed solution; and the mass ratio of the borax solution to the citric acid mixed solution in step Q3 is 0.7-1.4:1.

[0019] Further improvement, when the material A and the material B are simultaneously injected into the coal seam exploration hole by a peristaltic pump, the pumping speed ratio is 7-8: 1. If the pumping speeds of the material A and the material B do not match, local gelation will occur during the pumping process, which will eventually affect the gel effect of the sealing material.

[0020] The mixed sealing principle of material A and material B of the present invention is: sodium silicate and PVA components in material A, and citric acid and borax components in material B are used to form a sodium silicate-citric acid and PVA-borax dual coagulation mechanism, wherein the coagulation of sodium silicate-citric acid is similar to a rigid structure of cement properties, and the PVA-borax is coagulated into a mesh-like "soft steel bar" structure with certain flexibility, and then the xanthan gum in material A is used to improve the toughness and retain moisture, and the sodium chloride and matting powder in material B are used to improve the strength, so that material A and material B can be mixed in a required proportion and then gelled automatically within a controllable time, the gelation time is appropriate, the pressure resistance effect is excellent, and no obvious shrinkage occurs, so as to achieve the plugging effect of the coal seam exploration hole.

[0021] As another improvement of the present invention, the present invention also provides a method for preparing the above-mentioned coal seam exploration hole sealing material to form separately stored material A and material B. When in use, the material A and material B are simultaneously injected into the coal seam exploration hole at a certain speed ratio through a peristaltic pump to achieve rapid plugging of the exploration hole.

[0022] After adopting such a design, the present invention has at least the following advantages:

[0023] The coal seam exploration hole sealing material of the present invention is prepared by pre-configuring material A and material B, utilizing the dual coagulation mechanism of sodium silicate-citric acid and PVA-borax in material A and material B, and supplemented with xanthan gum to improve toughness and retain moisture, and sodium chloride and matting powder to improve strength. It only needs to match and set the pump speed during construction and pump it into the exploration hole at the same time. It can gel and seal itself within a certain period of time. It has the advantages of safety, environmental protection, low cost, controllable gel time, high hardness and toughness, excellent sealing effect, convenient construction, etc. It effectively solves the problem of negative pressure gas extraction in existing coal seam exploration and mining, reduces the risk factor, improves exploration and mining safety, and meets the requirements for later utilization of gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The above is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0025] Figure 1 The present invention is a schematic diagram of the structure of the device used for detecting the gel effect of the coal seam exploration hole sealing material. DETAILED DESCRIPTION

[0026] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0027] Embodiment 1:

[0028] Preparation material A:

[0029] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0030] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0031] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0032] Preparation material B:

[0033] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0034] (2) preparing a 30% concentration of citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0035] (3) The borax solution and the citric acid mixed solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0036] Embodiment 2:

[0037] Preparation material A:

[0038] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=5.7:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 15%;

[0039] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0040] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 4:1:4:0.5 (wt).

[0041] Preparation material B:

[0042] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0043] (2) preparing a 30% concentration citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1.3:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0044] (3) The borax solution and the citric acid mixed solution were mixed and stirred in a ratio of 0.7:1.2 (wt) to obtain material B.

[0045] Embodiment 3:

[0046] Preparation material A:

[0047] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0048] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0049] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0050] Preparation material B:

[0051] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0052] (2) preparing a 30% concentration citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.2 (wt%), and stirring to obtain a citric acid mixed solution;

[0053] (3) The borax solution and the citric acid mixed solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0054] Embodiment 4:

[0055] Preparation material A:

[0056] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0057] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water: xanthan gum powder = 5.7:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 15% is obtained;

[0058] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0059] Preparation material B:

[0060] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0061] (2) preparing a 30% concentration of citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0062] (3) The borax solution and the citric acid mixed solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0063] Embodiment 5:

[0064] Preparation material A:

[0065] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0066] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0067] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0068] Preparation material B:

[0069] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.05:0.025 (wt), stir and dissolve to prepare a 5% uniformly dispersed borax solution;

[0070] (2) preparing a 30% concentration of citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0071] (3) The borax solution and the citric acid mixed solution were mixed and stirred in a ratio of 1.4:1 (wt) to obtain material B.

[0072] Comparative Example 1:

[0073] Preparation material A:

[0074] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0075] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 19:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 5% is obtained;

[0076] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0077] Preparation material B:

[0078] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0079] (2) preparing a 30% concentration of citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0080] (3) The borax solution and the citric acid mixed solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0081] Comparative Example 2:

[0082] Preparation material A:

[0083] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0084] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0085] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0086] Preparation material B:

[0087] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0088] (2) preparing a 30% concentration of citric acid solution, adding sodium chloride solid and low pore volume matting powder in the ratio of citric acid solution: sodium chloride solid: low pore volume matting powder (using Sai De K02 matting powder) in sequence in the ratio of 1:0.2:0.1 (wt%), and stirring to obtain a citric acid mixed solution;

[0089] (3) The borax solution and the citric acid mixed solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0090] Comparative Example 3:

[0091] Preparation material A:

[0092] (1) Weigh a certain amount of pure water, heat it to 60°C, slowly add PVA powder (PVA203 produced by Kuraray, Japan) in a ratio of water:PVA=4:1 (wt), start stirring while adding, heat it to 90°C after adding, keep it warm and dissolve it, and after 1.5 hours, obtain a uniformly dispersed PVA solution with a concentration of 20%;

[0093] (2) Weigh a certain amount of pure water, heat it to 60° C., slowly add xanthan gum powder in a ratio of water to xanthan gum powder = 9:1 (wt), and stir while adding. After the addition is completed, heat it to 100° C. to keep it warm and dissolve. After 1 hour, a uniformly dispersed xanthan gum solution with a concentration of 10% is obtained;

[0094] (3) Weigh a certain amount of 20% sodium silicate solution, add water, PVA glue solution, and the newly prepared xanthan gum solution under continuous stirring to form material A. The mass ratio of sodium silicate solution, water, PVA solution, and xanthan gum solution is 3:1:4:0.5 (wt).

[0095] Preparation material B:

[0096] (1) Weigh a certain amount of pure water, add borax and glycerol in the ratio of water: borax: glycerol = 1:0.1:0.05 (wt%), stir and dissolve to prepare a 10% uniformly dispersed borax solution;

[0097] (2) preparing a 30% concentration of citric acid solution;

[0098] (3) The borax solution and the citric acid solution are mixed and stirred in a ratio of 0.7:1 (wt) to obtain material B.

[0099] Detection Example

[0100] The materials A and B obtained in the above examples 1 to 5 and comparative examples 1 to 3 were respectively pumped into the U-shaped airtightness detection device by a peristaltic pump device at a certain pump speed ratio, and the mixed gel of the materials A and B was observed during the pumping process, and the airtightness stability test was performed after the sealing material solidified, and the shrinkage of the sealing material after solidification was observed by visual inspection. The results are shown in Table 1 below.

[0101] The U-shaped air tightness detection device adopts a U-shaped tube 1 made of transparent material, as shown in the attached Figure 1 As shown, the P1 end of the U-shaped tube 1 is the sealing material pumping end, and the P2 end of the U-shaped device is the gas sealing end. The gas sealing end has a gas inlet 2 and a pressure gauge 3. A sealing valve (not shown) is provided at the gas inlet 2 to seal the gas sealing end after the gas is filled. The gas in the detection method can be methane gas or nitrogen, and the sealing effect of the sealing material after solidification is verified by detecting the pressure stability of the gas inside the gas sealing end.

[0102] Table 1 Airtight stability test results

[0103]

[0104] As can be seen from the results of Table 1 above, the material A and material B obtained in Examples 1 to 5 are based on the 7:1-8:1 pump speed ratio, and after being pumped into the U-shaped air tightness detection device at the same time, their pressure resistance stability can be greater than 30 days, and the volume shrinkage of the sealing material is all slight. Wherein, Example 1 obtains material A and material B, and at a pump speed ratio of 8:1, can obtain better pressure resistance, high tolerance stability and preferred gel time, indicating that its sealing effect is the best. And in Comparative Example 1, due to the reduction of the ratio of xanthan gum, the gel time of the sealing material is shortened, the pressure resistance is reduced, and the pressure resistance is especially stable for only 7 days, and the obvious shrinkage of volume can be seen within 7 days. In Comparative Example 2, due to the pump speed ratio of material A to material B being only 5:1, gel phenomenon occurred during the pumping process, resulting in the final sealing material being not pressure-resistant, and the exploration hole sealing effect cannot be achieved. In Comparative Example 3, due to the lack of sodium chloride and matting powder in material B, the strength of the sealing material is reduced, and the number of days of pressure resistance is reduced.

[0105] It can be seen from the above that the sealing material of the present invention needs to be based on the specific components and proportions of material A and material B, combined with a specific pump speed ratio, in order to meet the sealing requirements of coal seam exploration borehole plugging.

[0106] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Those skilled in the art may make some simple modifications, equivalent changes or modifications using the technical contents disclosed above, which all fall within the protection scope of the present invention.

Claims

1. A coal seam exploration hole sealing material, characterized in that: It includes material A and material B, wherein the material A and material B are configured and stored separately, and when used, they are simultaneously injected into the coal seam exploration hole through a peristaltic pump to achieve exploration hole plugging; The material A is a mixture of PVA, xanthan gum, sodium silicate and water; the material B is a mixture of borax, citric acid and water.

2. The coal seam exploration hole sealing material according to claim 1, characterized in that: The preparation method of the material A is: S1: Slowly add PVA powder into warm water at 50-80°C while stirring continuously, and keep warm at 90°C for 1-2h to obtain a completely dispersed PVA solution; S2: Slowly add the xanthan gum powder into warm water at 50-70°C while stirring continuously. After the addition is completed, continue stirring at 100°C for 15-30 minutes to obtain a xanthan gum solution; S3: Add the xanthan gum solution, the PVA solution and water just prepared into the sodium silicate solution under constant stirring to obtain the material A.

3. The coal seam exploration hole sealing material according to claim 2, characterized in that: The configuration concentration of the PVA solution in step S1 is 15-20%, the configuration concentration of the xanthan gum solution in step S2 is 10-15%, the configuration concentration of the sodium silicate solution in step S3 is 20%-30%, and the mass ratio of the sodium silicate solution, water, PVA solution and xanthan gum solution in step S3 is 3-4:1:4:0.

5.

4. The coal seam exploration hole sealing material according to claim 3, characterized in that: The preparation method of the material B is: Q1: Add borax solid and glycerol into water to prepare borax solution; Q2: Prepare citric acid solution; Q3: Add the citric acid solution to the borax solution to obtain the material B.

5. The coal seam exploration hole sealing material according to claim 4, characterized in that: Sodium chloride and low-pore volume matting powder are also added into the citric acid solution.

6. The coal seam exploration hole sealing material according to claim 5, characterized in that: The concentration of the borax solution in step Q1 is 5-10%; the concentration of the citric acid solution in step Q2 is 30-50%, and the mass ratio of the citric acid solution to the added sodium chloride solid and the low pore volume matting powder is 1:0.2:0.1-0.2 to form a citric acid mixed solution; and the mass ratio of the borax solution to the citric acid mixed solution in step Q3 is 0.7-1.4:

1.

7. The coal seam exploration hole sealing material according to claim 6, characterized in that: When the material A and the material B are simultaneously injected into the coal seam exploration hole by a peristaltic pump, the pumping speed ratio is 7-8:

1.

8. A method for preparing a coal seam exploration hole sealing material, characterized in that: The sealing material is the coal seam exploration hole sealing material according to claim 1, The preparation method of the material A is: S1: Slowly add PVA powder into warm water at 50-80°C while stirring continuously, and keep warm at 90°C for 1-2h to obtain a completely dispersed PVA solution; S2: Slowly add the xanthan gum powder into warm water at 50-70°C while stirring continuously. After the addition is completed, continue stirring at 100°C for 15-30 minutes to obtain a xanthan gum solution; S3: adding the xanthan gum solution, the PVA solution and water just prepared into the sodium silicate solution under constant stirring to obtain the material A; The preparation method of the material B is: Q1: Add borax solid and glycerol into water to prepare borax solution; Q2: Prepare citric acid solution; Q3: Add the citric acid solution to the borax solution to obtain the material B.

9. The method for preparing the coal seam exploration hole sealing material according to claim 8, characterized in that: The configuration concentration of the PVA solution in step S1 is 15-20%, the configuration concentration of the xanthan gum solution in step S2 is 10-15%, the configuration concentration of the sodium silicate solution in step S3 is 20%-30%, and the mass ratio of the sodium silicate solution, water, PVA solution and xanthan gum solution in step S3 is 3-4:1:4:0.

5.

10. The method for preparing the coal seam exploration hole sealing material according to claim 9, characterized in that: The concentration of the borax solution in step Q1 is 5-10%; the concentration of the citric acid solution in step Q2 is 30-50%, and sodium chloride and low-pore volume matting powder are also added to the citric acid solution, and the mass ratio of the citric acid solution to the sodium chloride solid and the matting powder is 1:0.2:0.1-0.2; the mass ratio of the borax solution to the citric acid mixed solution in step Q3 is 0.7-1.4:1.