Preparation method of water-resistant straw stalk fiber / unsaturated polyester composite packaging material

By treating straw straw fibers with phytic acid and anhydrous calcium chloride and combining them with unsaturated polyester, the problems of insufficient water resistance and flame retardant properties in the prior art are solved, and straw straw fiber/unsaturated polyester composite materials are realized Efficient and environmentally friendly production, suitable for a variety of packaging applications.

CN119060515APending Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411311338.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art When preparing water-resistant bio-based straw packaging materials, water resistance and flame retardant properties are insufficient, and the processing process is complex, which affects the application range and environmental protection of the material.

Method used

The straw straw fiber is treated with phytic acid and anhydrous calcium chloride. Through the flame retardant properties and chelating ability of phytic acid, it forms a stable complex with calcium ions, enhances the fiber binding force, and is compounded with unsaturated polyester to form a stable complex with Straw straw fiber/unsaturated polyester composite material with excellent water resistance and flame retardant properties.

Benefits of technology

It significantly improves the water resistance and flame retardant properties of composite materials, reduces production costs and energy consumption, is suitable for packaging fields with high moisture resistance requirements, and broadens the application range of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060515A_ABST
    Figure CN119060515A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a water-resistant straw stalk fiber / unsaturated polyester composite packaging material, which is characterized in that phytic acid and calcium ions in anhydrous calcium chloride form a stable phytic acid calcium complex mainly through the natural flame-retardant characteristic and strong chelation capability of phytic acid, and the phytic acid calcium complex and calcium ions in anhydrous calcium chloride jointly act on straw stalk fibers, so that the water-resistant straw stalk fiber / unsaturated polyester composite packaging material is prepared. The interface bonding force between the fiber and the polyester matrix is enhanced, and the composite material is prepared from the fiber and unsaturated polyester. And a flame-retardant layer can be formed during combustion under the carbonization action of phosphorus-containing groups in the modified phytic acid-calcium-straw fibers, so that the composite material is endowed with excellent flame-retardant property. Meanwhile, calcium ions, phytic acid and hydroxyl groups of straw fibers are subjected to complexation and coordination reaction, so that hydrophilic groups in a system are reduced, and the water resistance and mechanical properties of the composite material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bio-based straw composite packaging materials, and in particular relates to a method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material. Background Art

[0002] In the current context of rising demand for environmentally friendly and sustainable materials, bio-based packaging materials have attracted much attention due to their renewable and degradable properties. In view of the environmental pollution problems caused by traditional petroleum-based packaging materials such as plastics and foams, it is particularly urgent to seek environmentally friendly and economical alternative materials. As an agricultural by-product, rice straw has rich resources and renewable potential. The natural polymers such as cellulose, hemicellulose and lignin contained in it have the physical properties of low density and high specific strength, making it the preferred choice for manufacturing lightweight and high-strength packaging materials.

[0003] However, untreated straw fibers have strong hydrophilicity and poor compatibility with polymer matrices, which leads to increased water absorption of composite materials, thus affecting the water resistance of the materials and limiting the application of straw fibers in the packaging field. Therefore, the development of straw packaging materials with excellent water resistance stability, flame retardancy and mechanical properties is crucial to promote the development of green packaging materials.

[0004] Existing patent technologies still need to be optimized in the preparation of water-resistant bio-based straw packaging materials. For example, patent publication number CN112920567A enhances the environmental protection characteristics of the material by filling modified PLA fully degradable plastic with wheat straw, but it is still insufficient in terms of water resistance and flame retardancy. Patent publication number CN116985235A improves the mechanical properties of straw-based packaging materials through a dry preparation process, using degradable polymer adhesives and alkali lignin, but there are still limitations in water resistance. Patent publication number CN112980208A proposes a method of using a mixture of wheat straw fiber and polypropylene, adding a compatibilizing agent and a nano-toughness material, and successfully preparing a composite material for household daily necessities and imitation wood products. This technology has made significant progress in improving the compatibility of straw and plastics and enhancing mechanical properties, but its main focus is on improving the mechanical properties of the material, and the water resistance of the material has not been fully explored.

[0005] Phytic acid is a compound derived from natural plants. It has excellent biocompatibility and flame retardant properties. It can effectively avoid the environmental hazards caused by petroleum-based flame retardants. It also has strong chelating ability and can form stable complexes with metal ions. Patent publication number CN117820816A discloses a flame-retardant and easily degradable epoxy resin precursor, in which calcium phytate is a key component to enhance the flame retardancy of the material. Patent publication number CN118006038A discloses a flame-retardant polypropylene composite material for automotive interior parts. It uses calcium phytate, magnesium hybrid and lignin composite flame retardants, and adds toughening agents, antioxidants and other ingredients to jointly improve the flame retardant and mechanical properties of polypropylene materials. Patent publication number CN118459944A discloses a lignin-based flame-retardant biodegradable PBAT composite material and its preparation method. By combining phytic acid-metal ion modified lignin powder with PBAT resin and antioxidants, a biodegradable composite material with flame retardant properties is prepared. Although these methods demonstrate the potential of phytic acid and its derivatives in improving material properties, they mainly focus on their single flame retardant property, and patents on their use as water-resistant modification of straw fibers have not yet been found. Summary of the invention

[0006] In order to solve the above-mentioned technical problems existing in the prior art, the present application aims to study the application of phytic acid and its derivatives in bio-based composite packaging materials, and to enhance the water resistance of straw fiber / unsaturated polyester composite materials by using phytic acid and anhydrous calcium chloride as functional modifiers of rice straw fiber, while giving them good flame retardant properties and certain mechanical properties.

[0007] Specifically, the present invention provides the following technical solutions:

[0008] As a first aspect of the present invention, a method for jointly treating rice straw fibers using phytic acid and anhydrous calcium chloride is proposed. This method not only forms a stable complex with calcium ions through the natural flame retardant properties and chelating ability of phytic acid to enhance the fiber binding force, but also effectively improves the water resistance and flame retardant properties of the composite material by coordinating calcium ions with the hydroxyl groups of straw fibers.

[0009] Furthermore, the method of the present invention comprises the following steps:

[0010] S1: treating rice straw fibers with a length of 5 to 20 mm with a phytic acid aqueous solution, allowing the rice straw fibers to fully absorb the phytic acid aqueous solution and then taking them out and drying them for not less than 8 hours to obtain phytic acid-straw fibers;

[0011] S2: mixing a calcium chloride aqueous solution with phytic acid-straw fiber, stirring and reacting for a certain period of time, and then drying for not less than 8 hours to obtain phytic acid-calcium-straw fiber;

[0012] Preferably, the mass content of phytic acid in step S1 is 10% to 20%, and the mass: volume ratio of rice straw fiber to phytic acid aqueous solution is 1:1 to 2:3. The mass content of calcium chloride in step S2 is 15% to 25%, and the reaction time is 1 to 2 hours.

[0013] As a second aspect of the present invention, a method for preparing a rice straw fiber / unsaturated polyester composite material is provided. The method does not require complicated equipment, is easy to operate, is suitable for large-scale production, and meets the requirements of green chemical industry.

[0014] Furthermore, the method for preparing the rice straw fiber / unsaturated polyester composite material is: phytic acid-calcium-straw fiber is uniformly mixed with unsaturated polyester containing tert-butyl perbenzoate, and the mixture is placed in a mold and heated and cured to obtain the rice straw fiber / unsaturated polyester composite material.

[0015] Furthermore, in step S3, based on the mass of the unsaturated polyester being 100%, the amount of phytic acid-calcium-straw fiber is in the range of 20% to 100%, and the amount of tert-butyl perbenzoate is in the range of 4% to 6%.

[0016] Furthermore, the curing conditions in step S3 are: temperature of 100-120° C. and time of 1-2 hours.

[0017] The present invention forms a stable calcium phytate complex with calcium ions in anhydrous calcium chloride through the strong chelating ability of phytic acid and the carbonization of phosphorus-containing groups, acts on rice straw fibers together, and then prepares a composite material with unsaturated polyester. The calcium ions react with phytic acid and hydroxyl groups of the straw fibers to form a complex and coordinate reaction, thereby reducing the hydrophilic groups in the system, enhancing the interfacial bonding force between the straw fibers and the polyester matrix, and effectively improving the water resistance and mechanical properties of the composite material. At the same time, the carbonization of the phosphorus-containing groups in the phytic acid-calcium-straw fibers forms a flame retardant layer during combustion, giving the composite material excellent flame retardant properties.

[0018] The present invention transforms agricultural waste into products with economic and social value. With its simple and efficient process flow and excellent water resistance, it provides new ideas and solutions for the sustainable development of bio-based composite packaging materials, promotes the green transformation of the packaging industry, and makes positive contributions to the development of the circular economy.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] (i) The composite material of the present invention has excellent water resistance. In the water resistance test, its water absorption rate is 5.9% and its thickness expansion rate is 1.76%, which is better than the existing related patents. Therefore, the composite material is particularly suitable for packaging fields such as food, medicine and electronic products with extremely high moisture resistance requirements, and can effectively resist erosion in humid environments.

[0021] (ii) The rice straw fiber used in the present invention does not need to be subjected to complicated pre-treatment, and can be directly used in the preparation of the composite material by simply rolling and cutting into 5 to 20 mm, without the need for a crushing process. This simplified processing flow not only reduces the difficulty of material preparation, but also reduces energy consumption and the demand for equipment, making the entire production process more efficient and economical.

[0022] (iii) The modification process of straw fiber in the present invention is green, environmentally friendly and low-cost. Compared with other methods, no additional rinsing step is required, thereby reducing water resource consumption and production costs, while also reducing the discharge of chemical waste, successfully achieving the green and environmentally friendly production goal.

[0023] (iv) The composite material of the present invention has remarkable multifunctionality. It not only has excellent water resistance, but also has good flame retardant properties and certain mechanical strength. The comprehensive presentation of these functions makes the material not only suitable for the traditional packaging field, but also has the potential to be widely used in occasions with higher material performance requirements, such as building material packaging, flammable goods transportation, etc., which greatly broadens the application scope of straw composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figure is a schematic diagram of the process flow of the modification and preparation method of straw fiber.

[0025] Figure 2 The figure is a schematic diagram of the process for preparing rice straw fiber / unsaturated polyester composite materials. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0027] The water resistance test involved in the present invention is a result obtained by immersing the composite material in 80° C. water for 168 hours in accordance with the standard HB 7401-2021 “Test method for moisture absorption of polymer-based composite materials for aviation use”.

[0028] As shown in Table 1 and Table 2, Examples 1 to 13 achieved excellent water resistance, while Comparative Examples 14 to 31 failed to achieve excellent water resistance.

[0029] Example 1

[0030] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0031] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0032] 4 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-1.

[0033] The water contact angle of the obtained sample PCRU-1 decreased from 84.3° to 61.7° within 6 minutes, the water absorption rate was 6.07%, the thickness expansion rate was 2.13%, the tensile strength was 11.37 MPa, and the limiting oxygen index was 28.9%.

[0034] Example 2

[0035] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0036] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0037] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-2.

[0038] The water contact angle of the obtained sample PCRU-2 decreased from 87.5° to 64.4° within 6 minutes, the water absorption rate was 5.90%, the thickness expansion rate was 1.76%, the tensile strength was 12.04 MPa, and the limiting oxygen index was 29.7%.

[0039] Example 3

[0040] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0041] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0042] 8 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-3.

[0043] The water contact angle of the obtained sample PCRU-3 decreased from 88.1° to 63.6° within 6 minutes, the water absorption rate was 6.20%, the thickness expansion rate was 2.17%, the tensile strength was 11.15 MPa, and the limiting oxygen index was 28.3%.

[0044] Example 4

[0045] 10 grams of rice straw fiber and 15 milliliters of 10% by mass phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0046] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0047] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-4.

[0048] The water contact angle of the obtained sample PCRU-4 decreased from 85.4° to 62.2° within 6 minutes, the water absorption rate was 6.07%, the thickness expansion rate was 1.83%, the tensile strength was 11.81 MPa, and the limiting oxygen index was 28.5%.

[0049] Example 5

[0050] 10 grams of rice straw fiber and 15 milliliters of phytic acid aqueous solution with a mass content of 20% were uniformly stirred. After the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0051] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0052] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-5.

[0053] The water contact angle of the obtained sample PCRU-5 decreased from 85.1° to 60.7° within 6 minutes, the water absorption rate was 6.18%, the thickness expansion rate was 2.03%, the tensile strength was 11.34 MPa, and the limiting oxygen index was 29.8%.

[0054] Example 6

[0055] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0056] The phytic acid-straw fiber was immersed in 50 ml of a 15% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0057] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-6.

[0058] The water contact angle of the obtained sample PCRU-6 decreased from 83.9° to 60.0° within 6 minutes, the water absorption rate was 6.23%, the thickness expansion rate was 2.15%, the tensile strength was 11.05 MPa, and the limiting oxygen index was 28.1%.

[0059] Example 7

[0060] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0061] The phytic acid-straw fiber was immersed in 50 ml of a 25% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0062] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-7.

[0063] The water contact angle of the obtained sample PCRU-7 decreased from 88.7° to 65.1° within 6 minutes, the water absorption rate was 5.84%, the thickness expansion rate was 1.82%, the tensile strength was 11.98 MPa, and the limiting oxygen index was 28.7%.

[0064] Example 8

[0065] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0066] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 2 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0067] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-8.

[0068] The water contact angle of the obtained sample PCRU-8 decreased from 85.1° to 70.6° within 6 minutes, the water absorption rate was 6.01%, the thickness expansion rate was 1.99%, the tensile strength was 10.97 MPa, and the limiting oxygen index was 27.9%.

[0069] Example 9

[0070] 10 grams of rice straw fiber and 10 milliliters of 15% by mass phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0071] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0072] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-9.

[0073] The water contact angle of the obtained sample PCRU-9 decreased from 85.5° to 63.7° within 6 minutes, the water absorption rate was 6.11%, the thickness expansion rate was 2.07%, the tensile strength was 11.57 MPa, and the limiting oxygen index was 28.8%.

[0074] Example 10

[0075] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0076] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0077] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.6 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain a sample PCRU-10.

[0078] The water contact angle of the obtained sample PCRU-10 decreased from 87.3° to 63.2° within 6 minutes, the water absorption rate was 6.02%, the thickness expansion rate was 1.83%, the tensile strength was 11.51 MPa, and the limiting oxygen index was 29.1%.

[0079] Embodiment 11

[0080] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0081] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0082] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 100° C. for 2 hours to obtain sample PCRU-11.

[0083] The water contact angle of the obtained sample PCRU-11 decreased from 86.5° to 63.4° within 6 minutes, the water absorption rate was 6.19%, the thickness expansion rate was 2.11%, the tensile strength was 11.32 MPa, and the limiting oxygen index was 28.9%.

[0084] Example 12

[0085] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0086] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0087] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 1 hour to obtain sample PCRU-12.

[0088] The water contact angle of the obtained sample PCRU-12 decreased from 85.3° to 66.5° within 6 minutes, the water absorption rate was 5.97%, the thickness expansion rate was 1.90%, the tensile strength was 11.24 MPa, and the limiting oxygen index was 28.7%.

[0089] Example 13

[0090] 1200 g of rice straw fiber and 1800 ml of phytic acid aqueous solution with a mass content of 15% were uniformly stirred. After the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0091] The phytic acid-straw fiber was immersed in 5000 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0092] 1125 g of phytic acid-calcium-straw fiber, 1875 g of unsaturated polyester and 7.5 g of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-13.

[0093] The water contact angle of the obtained sample PCRU-13 decreased from 86.7° to 62.8° within 6 minutes, the water absorption rate was 5.99%, the thickness expansion rate was 1.84%, the tensile strength was 12.59 MPa, and the limiting oxygen index was 29.5%.

[0094] Comparative Example 14

[0095] 10 grams of unsaturated polyester, 0.4 grams of tert-butyl perbenzoate and 6 grams of rice straw fiber were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample RU-14.

[0096] The water contact angle of the obtained sample RU-14 decreased from 77.6° to 53.6° within 6 minutes, the water absorption rate was 12.51%, the thickness expansion rate was 12.62%, and the tensile strength was 10.83 MPa.

[0097] Comparative Example 15

[0098] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0099] 6 g of phytic acid-straw fiber, 10 g of unsaturated polyester and 0.4 g of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PRU-15.

[0100] The water contact angle of the obtained sample PRU-15 decreased from 47.3° to 0° within 6 minutes, the water absorption rate was 23.72%, the thickness expansion rate was 3.77%, the tensile strength was 8.26 MPa, and the limiting oxygen index was 19.3%.

[0101] In Comparative Examples 14 to 15, the rice straw fiber was not modified by using phytic acid and anhydrous calcium chloride, resulting in the composite material not having certain water resistance.

[0102] Comparative Example 16

[0103] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0104] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0105] 2 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-16.

[0106] The water contact angle of the obtained sample PCRU-16 decreased from 80.3° to 58.7° within 6 minutes, the water absorption rate was 8.73%, the thickness expansion rate was 3.26%, the tensile strength was 9.01 MPa, and the limiting oxygen index was 25.2%.

[0107] Comparative Example 17

[0108] 14 grams of rice straw fiber and 21 milliliters of 15% by mass phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0109] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0110] 10 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-17.

[0111] The water contact angle of the obtained sample PCRU-17 decreased from 90.5° to 65.1° within 6 minutes, the water absorption rate was 6.57%, the thickness expansion rate was 2.47%, the tensile strength was 11.01 MPa, and the limiting oxygen index was 28.8%.

[0112] In Comparative Examples 16-17, when the amount of unsaturated polyester is too low, the fiber content in the composite material is too high, the water absorption is enhanced, and the water resistance of the material is reduced. On the contrary, when the amount of unsaturated polyester is too high, the polyester content is relatively high, resulting in poor water resistance of the composite material.

[0113] Comparative Example 18

[0114] 10 grams of rice straw fiber and 15 milliliters of a phytic acid aqueous solution with a mass content of 5% were uniformly stirred. After the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0115] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0116] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-18.

[0117] The water contact angle of the obtained sample PCRU-18 decreased from 83.7° to 60.6° within 6 minutes, the water absorption rate was 6.41%, the thickness expansion rate was 2.37%, the tensile strength was 9.35 MPa, and the limiting oxygen index was 26.9%.

[0118] Comparative Example 19

[0119] 10 grams of rice straw fiber and 15 milliliters of phytic acid aqueous solution with a mass content of 25% were evenly stirred. After the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0120] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0121] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-19.

[0122] The water contact angle of the obtained sample PCRU-19 decreased from 84.3° to 59.9° within 6 minutes, the water absorption rate was 6.35%, the thickness expansion rate was 2.44%, the tensile strength was 10.07 MPa, and the limiting oxygen index was 29.1%.

[0123] In Comparative Examples 18-19, when the concentration of the phytic acid aqueous solution is too low, the straw fiber absorbs too little phytic acid, affecting the formation of the phytic acid-calcium complex, resulting in insufficient modification. If the concentration of the phytic acid aqueous solution is too high, excessive phytic acid will also cause the water resistance of the composite material to decrease.

[0124] Comparative Example 20

[0125] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0126] The phytic acid-straw fiber was immersed in 50 ml of a 10% calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0127] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain a sample PCRU-20.

[0128] The water contact angle of the obtained sample PCRU-20 decreased from 80.5° to 59.3° within 6 minutes, the water absorption rate was 6.51%, the thickness expansion rate was 2.76%, the tensile strength was 10.57 MPa, and the limiting oxygen index was 27.1%.

[0129] Comparative Example 21

[0130] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0131] The phytic acid-straw fiber was immersed in 50 ml of a 30% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0132] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-21.

[0133] The water contact angle of the obtained sample PCRU-21 decreased from 90.1° to 70.4° within 6 minutes, the water absorption rate was 6.32%, the thickness expansion rate was 2.37%, the tensile strength was 10.59 MPa, and the limiting oxygen index was 27.6%.

[0134] Comparative Example 22

[0135] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0136] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 1 hour, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0137] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-22.

[0138] The water contact angle of the obtained sample PCRU-22 decreased from 83.7° to 68.7° within 6 minutes, the water absorption rate was 6.25%, the thickness expansion rate was 2.19%, the tensile strength was 9.99 MPa, and the limiting oxygen index was 26.1%.

[0139] Comparative Example 23

[0140] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0141] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 4 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0142] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-23.

[0143] The water contact angle of the obtained sample PCRU-23 decreased from 86.7° to 72.3° within 6 minutes, the water absorption rate was 6.27%, the thickness expansion rate was 2.15%, the tensile strength was 10.31 MPa, and the limiting oxygen index was 26.9%.

[0144] In Comparative Examples 20 to 23, when the concentration of the calcium chloride aqueous solution is too low or the reaction time is too short, insufficient complexes are formed on the fiber surface, resulting in increased water absorption. On the contrary, too high a concentration or a long reaction time will result in excessive deposition of calcium chloride on the fiber surface, affecting the composite of the fiber and the unsaturated polyester, resulting in poor overall performance of the composite material.

[0145] Comparative Example 24

[0146] 10 grams of rice straw fiber and 20 milliliters of 15% by mass phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0147] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0148] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-24.

[0149] The water contact angle of the obtained sample PCRU-24 decreased from 83.5° to 60.4° within 6 minutes, the water absorption rate was 6.31%, the thickness expansion rate was 2.35%, the tensile strength was 10.64 MPa, and the limiting oxygen index was 27.9%.

[0150] Comparative Example 25

[0151] 10 grams of rice straw fiber and 5 milliliters of 15% by mass phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0152] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0153] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain a sample PCRU-25.

[0154] The water contact angle of the obtained sample PCRU-25 decreased from 86.9° to 60.1° within 6 minutes, the water absorption rate was 6.64%, the thickness expansion rate was 2.47%, the tensile strength was 9.94 MPa, and the limiting oxygen index was 26.4%.

[0155] In comparative examples 24-25, according to research data, the water absorption of rice straw can reach 427.9% of its own weight. Therefore, the ratio of straw fiber to phytic acid aqueous solution also needs to be precisely controlled. If the ratio is too high, the straw fiber will not absorb enough; if the ratio is too low, the fiber surface will absorb too many hydrophilic groups, thereby reducing the water resistance of the composite material.

[0156] Comparative Example 26

[0157] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0158] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0159] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.2 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-26.

[0160] The water contact angle of the obtained sample PCRU-26 decreased from 85.7° to 62.1° within 6 minutes, the water absorption rate was 6.22%, the thickness expansion rate was 2.35%, the tensile strength was 9.51 MPa, and the limiting oxygen index was 25.9%.

[0161] Comparative Example 27

[0162] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0163] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0164] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.8 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 2 hours to obtain sample PCRU-27.

[0165] The water contact angle of the obtained sample PCRU-27 decreased from 86.4° to 62.9° within 6 minutes, the water absorption rate was 6.27%, the thickness expansion rate was 2.09%, the tensile strength was 10.33 MPa, and the limiting oxygen index was 27.6%.

[0166] In Comparative Examples 26-27, too little initiator usage will result in incomplete curing, while too much initiator usage will cause the material to become more brittle and prone to cracking, both of which will affect the comprehensive performance of the composite material.

[0167] Comparative Example 28

[0168] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0169] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0170] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 80° C. for 2 hours to obtain sample PCRU-28.

[0171] The water contact angle of the obtained sample PCRU-28 decreased from 82.1° to 57.6° within 6 minutes, the water absorption rate was 7.01%, the thickness expansion rate was 2.68%, the tensile strength was 9.12 MPa, and the limiting oxygen index was 25.7%.

[0172] Comparative Example 29

[0173] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0174] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0175] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 140° C. for 2 hours to obtain sample PCRU-29.

[0176] The water contact angle of the obtained sample PCRU-29 decreased from 87.1° to 63.7° within 6 minutes, the water absorption rate was 6.27%, the thickness expansion rate was 2.22%, the tensile strength was 10.54 MPa, and the limiting oxygen index was 29.1%.

[0177] Comparative Example 30

[0178] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0179] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0180] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 0.5 hours to obtain a sample PCRU-30.

[0181] The water contact angle of the obtained sample PCRU-30 decreased from 83.5° to 59.4° within 6 minutes, the water absorption rate was 6.84%, the thickness expansion rate was 2.55%, the tensile strength was 11.10 MPa, and the limiting oxygen index was 26.7%.

[0182] Comparative Example 31

[0183] 10 grams of rice straw fiber and 15 milliliters of 15% phytic acid aqueous solution were uniformly stirred, and after the rice straw fiber fully absorbed the phytic acid aqueous solution, it was dried at 80° C. for 8 hours to obtain phytic acid-straw fiber.

[0184] The phytic acid-straw fiber was immersed in 50 ml of a 20% by mass calcium chloride aqueous solution, stirred evenly for reaction for 3 hours, and then dried at 80° C. for 8 hours to obtain the phytic acid-calcium-straw fiber.

[0185] 6 grams of phytic acid-calcium-straw fiber, 10 grams of unsaturated polyester and 0.4 grams of tert-butyl perbenzoate were uniformly mixed and placed in a mold, and heated and cured at 120° C. for 3 hours to obtain sample PCRU-31.

[0186] The water contact angle of the obtained sample PCRU-31 decreased from 87.5° to 64.2° within 6 minutes, the water absorption rate was 6.22%, the thickness expansion rate was 2.19%, the tensile strength was 11.01 MPa, and the limiting oxygen index was 28.1%.

[0187] In Comparative Examples 28 to 31, the curing temperature is too low or the curing time is insufficient, which will result in incomplete curing of the composite material. If the curing temperature is too high or the curing time is too long, excessive stress will be generated inside the composite material, causing the material to become brittle, which will also affect the performance of the composite material.

[0188]

[0189]

[0190] Table 1. Preparation conditions of rice straw fiber / unsaturated polyester composites.

[0191]

[0192]

[0193] Table 2. Characterization results of composite materials properties of various embodiments and comparative examples.

Claims

1. A method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material, characterized in that: The following steps are involved: S1: treating rice straw fibers with a length of 5 to 20 mm with a phytic acid aqueous solution, allowing the rice straw fibers to fully absorb the phytic acid aqueous solution, and then taking them out and drying them for not less than 8 hours to obtain phytic acid-straw fibers; S2: mixing a calcium chloride aqueous solution with phytic acid-straw fiber, stirring and reacting for a certain period of time, and drying for not less than 8 hours to obtain phytic acid-calcium-straw fiber; S3: Evenly mix phytic acid-calcium-straw fiber with unsaturated polyester containing tert-butyl perbenzoate, place in a mold, heat and cure, and prepare a water-resistant rice straw fiber / unsaturated polyester composite material.

2. The method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material according to claim 1, characterized in that: The mass content of phytic acid in the phytic acid aqueous solution in step S1 is 10% to 20%, and the mass: volume ratio of the rice straw fiber to the phytic acid aqueous solution is 1:1 to 2:3 g / mL.

3. The method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material according to claim 1, characterized in that: The mass content of calcium chloride in the calcium chloride aqueous solution of step S2 is 15% to 25%, and the reaction time is 1 to 2 hours.

4. The method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material according to claim 1, characterized in that: In step S3, based on the mass of the unsaturated polyester being 100%, the amount of phytic acid-calcium-straw fiber is in the range of 20% to 100%, and the amount of tert-butyl perbenzoate is in the range of 4% to 6%.

5. The method for preparing a water-resistant rice straw fiber / unsaturated polyester composite packaging material according to claim 1, characterized in that: The curing conditions in step S3 are: temperature of 100-120° C. and time of 1-2 hours.