Modified polyphenyl ether, preparation method thereof and 5G base station material

The modified polyphenylene ether, blended with polystyrene and modified titanium dioxide, addresses the low dielectric constant and high dielectric loss issues, providing enhanced mechanical properties and performance for 5G base stations.

CN119060525APending Publication Date: 2024-12-03QINGDAO HAIER NEW MATERIAL R&D CO LTD +1

Patent Information

Application Number
CN202411348636.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The dielectric constant of polyphenylene ether is relatively low, and its dielectric loss increases during modification, failing to meet the mechanical and performance requirements of 5G base stations.

Method used

A modified polyphenylene ether is prepared by blending polyphenylene ether with polystyrene and adding a toughening agent, along with modified titanium dioxide, to achieve a stable dielectric constant and low dielectric loss, enhanced mechanical properties, and improved compatibility.

Benefits of technology

The modified polyphenylene ether exhibits a dielectric constant of 5-7 and dielectric loss of (0.8-0.9)*10^-3, with tensile strength of 50-70 MPa and bending strength of 90-110 MPa, suitable for 5G base station applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060525A_ABST
    Figure CN119060525A_ABST
Patent Text Reader

Abstract

The invention provides modified polyphenyl ether, a preparation method thereof and a 5G base station material, and belongs to the technical field of polymer modification. According to the invention, the polyphenyl ether is used as a main body, the polystyrene and the flexibilizer are added into the polyphenyl ether for modification, the polyphenyl ether, the polystyrene and the flexibilizer all contain double-bond structures, the compatibility is better, and the impact resistance and the tensile strength of the polyphenyl ether are also improved, in addition, the modified titanium dioxide is also added, and the titanium dioxide is an inorganic material, so that the impact resistance and the tensile strength of the polyphenyl ether are improved. The titanium dioxide has poor compatibility with an organic polymer, and after organic treatment and inorganic coating, the compatibility between the titanium dioxide and the organic polymer is improved, and the dielectric loss of polyphenyl ether is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer modification, and in particular to a modified polyphenylene ether and a preparation method thereof, and a 5G base station material. Background Art

[0002] 5G base stations are the core equipment of 5G networks, providing wireless coverage and realizing wireless signal transmission between wired communication networks and wireless terminals. 5G technology uses millimeter waves in the 26GHz to 40GHz spectrum for signal transmission. Under such high-frequency signal transmission, there will be obvious signal attenuation, which requires higher power and energy, and will generate more heat. In order to increase the transmission speed of 5G signals and reduce signal attenuation, it is necessary to select suitable materials for 5G base station materials. Polytetrafluoroethylene, liquid crystal polymers, ceramics and other organic polymers are often used as 5G base station materials. Among them, the organic polymer polyphenylene ether has been widely used in the 5G field because it can optimize the performance of 5G base station materials and has low dielectric constant and dissipation factor.

[0003] CN115850867B discloses a modified PP / PPO / GF-based composite dielectric material for high-frequency circuit boards, and relates to the technical field of circuit board materials. A modified PP / PPO / GF-based composite dielectric material for high-frequency circuit boards, the raw materials of which include, by mass, 7.9-37 parts of polypropylene; 3.4-15.8 parts of polyphenylene ether; 2.8-13.2 parts of glass fiber; 30-85 parts of CaTiO3 ceramic powder; and 0.9-4 parts of compounded compatibilizer. The present invention uses PP / PPO / GF as a base material to prepare a dielectric material, and by filling CaTiO3 ceramic powder with high dielectric constant and extremely low dielectric loss, and adding a compounded compatibilizer, the prepared modified PP / PPO / GF-based composite dielectric material has a continuously adjustable dielectric constant (3.14-20.9), a dielectric loss of less than 0.0021, and a Vicat softening temperature of more than 164°C. At the same time, it has excellent injection molding properties and mechanical properties, and can meet the requirements of 5G base station applications for high-frequency circuit boards.

[0004] CN111393828A discloses a low dielectric constant polyphenylene ether composition and a preparation method thereof, wherein the low dielectric constant polyphenylene ether composition is prepared from the following raw materials: polyphenylene ether resin, high impact polystyrene resin, polyphenylene ether grafted maleic anhydride, hydrogenated styrene-butadiene-styrene copolymer grafted maleic anhydride, hollow glass microspheres, polyhedral oligomeric silsesquioxane polymer, titanate coupling agent, polytetrafluoroethylene resin, hyperbranched polyester polymer, erucic acid amide, N, N'-bis (2,2,6,6-tetramethyl-4-piperidinyl) -1,3-benzenedicarbamide, bis (2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate. The low dielectric constant polyphenylene ether composition has excellent mechanical properties, processing properties and low dielectric constant, and can be applied to 5G base stations, micro base station systems, data communication terminals, shells and coatings of antennas and radio frequency modules, protective materials, etc.

[0005] Phase shifter is an essential component of 5G base station antenna. The dielectric plate in the phase shifter usually requires good dimensional stability, adjustable dielectric constant and extremely low dielectric loss. Polyphenylene ether resin (PPO) is a thermoplastic engineering plastic with excellent comprehensive performance. It has the lowest dielectric loss among engineering plastics, with a dielectric loss of 0.4*10 -3 . Moreover, its dielectric constant is almost unaffected by temperature and humidity. Therefore, it can be used in low, medium and high frequency electric field fields, and plays an important role in 5G base station phase shifters.

[0006] However, the dielectric constant of polyphenylene ether resin is relatively low, about 2.5, and fillers are usually required to be added to adjust the dielectric constant of the material after modification to meet the use requirements. However, the dielectric loss of polyphenylene ether will increase during the modification process, making the comprehensive performance of the modified polyphenylene ether unable to meet the use requirements, and the mechanical properties of polyphenylene ether cannot meet the requirements of 5G base stations.

[0007] In summary, the low dielectric loss of polyphenylene ether makes it suitable for 5G base station signal materials. However, due to the requirements of its application sites, the increased dielectric loss, small dielectric constant and mechanical properties of polyphenylene ether during the modification process cannot meet the requirements of 5G base stations, which are still urgent problems to be solved. Summary of the invention

[0008] In view of the above problems, the present invention provides a modified polyphenylene ether, a preparation method thereof and a 5G base station material. The modified polyphenylene ether prepared by blending and modifying polyphenylene ether and polystyrene, and adding modified titanium dioxide and a toughening agent for blending has a stable dielectric constant and low dielectric loss, as well as mechanical properties such as high impact strength and tensile strength.

[0009] The invention provides a modified polyphenylene ether. The modified polyphenylene ether is obtained by injection molding after the polyphenylene ether, polystyrene, a toughening agent, a modified titanium dioxide, an antioxidant and a lubricant are mixed and modified; the melt index of the modified polyphenylene ether at 300°C / 5kg is 9-15g / 10min, and the heat deformation temperature of 0.45MPa is 170-175°C; the tensile strength of the modified polyphenylene ether is 50-70MPa, the bending strength is 90-110MPa, and the 23°C simply supported beam notched impact strength is 6-8kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5-7, and the dielectric loss at 23°C is (0.8-0.9)*10 -3 ; The components and contents in the modified polyphenylene ether are: Polyphenylene ether: 20-40 parts by weight; Polystyrene: 5-15 parts by weight; Toughening agent: 5-15 parts by weight; Modified titanium dioxide: 35-60 parts by weight; Antioxidant: 0.3-2 parts by weight; Lubricant: 0.3-2 parts by weight.

[0010] Furthermore, the polyphenylene ether has a viscosity of one or more of 0.35±0.02 dL / g and 0.4±0.02 dL / g at 25°C.

[0011] Furthermore, the viscosity of the polyphenylene ether at 25°C is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-23000; the viscosity of the polyphenylene ether at 25°C is 0.4±0.02 dL / g, and the weight average molecular weight is 20000-25000.

[0012] Furthermore, the polystyrene has a melt index of 2-15 g / 10 min at 200° C. / 5 kg.

[0013] Furthermore, the toughening agent is styrene-butadiene-styrene copolymer (SEBS).

[0014] Furthermore, the preparation process of the modified titanium dioxide is as follows: At room temperature, inorganic nanoparticles are dispersed in deionized water to obtain an inorganic solution, which is then sprayed onto titanium dioxide with stirring, and then rinsed with deionized water and dried to obtain an inorganic coated titanium dioxide. The inorganic coated titanium dioxide and organic silane are stirred and mixed in a high mixing pot, and then dried after mixing to obtain the modified titanium dioxide.

[0015] Furthermore, the mass volume ratio of the inorganic nanoparticles to the deionized water is (10:0.15)-(10:0.2) g / L.

[0016] Furthermore, the stirring speed is 300-500r / min.

[0017] Furthermore, the mass ratio of the inorganic nanoparticles to the titanium dioxide is (1:5)-(1:6).

[0018] Furthermore, the inorganic nanoparticles are one or more of aluminum oxide and zirconium oxide.

[0019] Furthermore, the titanium dioxide is rutile titanium dioxide, specifically including spherical titanium dioxide and rod-shaped titanium dioxide, and the mass ratio of the spherical titanium dioxide to the rod-shaped titanium dioxide is (1:1)-(1:2.4).

[0020] Furthermore, the flushing is performed 3-5 times.

[0021] Furthermore, the drying temperature is 100-200° C., and the drying time is 2-3 hours.

[0022] Furthermore, the mass ratio of the titanium dioxide to the organosilane is (5:3)-(2:1).

[0023] Furthermore, the organosilane is γ-methacryloxypropyltrimethoxysilane.

[0024] Furthermore, the stirring and mixing speed is 300-500 r / min, the stirring and mixing temperature is 100-150° C., and the stirring and mixing time is 3-10 min.

[0025] Furthermore, the temperature of the drying after mixing is 100-150° C., and the time of the drying after mixing is 2-3 hours.

[0026] Furthermore, the antioxidant is a compound of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168) in a mass ratio of 1:2.

[0027] Furthermore, the lubricant is one or more of silicone powder, pentaerythritol stearate and stearamide.

[0028] The present invention also provides a method for preparing modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer and stirring to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch, add it into an injection molding machine for injection molding to obtain the modified polyphenylene ether.

[0029] Furthermore, in step 1, the mass ratio of the polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant is (20-40): (5-15): (5-15): (35-60): (0.3-2): (0.3-2).

[0030] Furthermore, the polyphenylene ether in step 1 has a viscosity of one or more of 0.35±0.02dL / g and 0.4±0.02dL / g at 25°C.

[0031] Furthermore, the weight average molecular weight of the polyphenylene ether having a viscosity of 0.35±0.02 dL / g at 25°C is 15000-23000; the weight average molecular weight of the polyphenylene ether having a viscosity of 0.4±0.02 dL / g at 25°C is 20000-25000.

[0032] Furthermore, in the step 1, the melt index of the polystyrene at 200°C / 5kg is 2-15g / 10min.

[0033] Furthermore, the toughening agent in step 1 is styrene-butadiene-styrene copolymer (SEBS).

[0034] Furthermore, the preparation process of the modified titanium dioxide in step 1 is: At room temperature, inorganic nanoparticles are dispersed in deionized water to obtain an inorganic solution, which is then sprayed onto titanium dioxide with stirring, and then rinsed with deionized water and dried to obtain an inorganic coated titanium dioxide. The inorganic coated titanium dioxide and organic silane are stirred and mixed in a high mixing pot, and then dried after mixing to obtain the modified titanium dioxide.

[0035] Furthermore, the mass volume ratio of the inorganic nanoparticles to the deionized water is (10:0.15)-(10:0.2) g / L.

[0036] Furthermore, the stirring speed is 300-500r / min.

[0037] Furthermore, the mass ratio of the inorganic nanoparticles to the titanium dioxide is (1:5)-(1:6).

[0038] Furthermore, the inorganic nanoparticles are one or more of aluminum oxide and zirconium oxide.

[0039] Furthermore, the titanium dioxide is rutile titanium dioxide, specifically including spherical titanium dioxide and rod-shaped titanium dioxide, and the mass ratio of the spherical titanium dioxide to the rod-shaped titanium dioxide is (1:1)-(1:2.4).

[0040] Furthermore, the flushing is performed 3-5 times.

[0041] Furthermore, the drying temperature is 100-200° C., and the drying time is 2-3 hours.

[0042] Furthermore, the mass ratio of the titanium dioxide to the organosilane is (5:3)-(2:1).

[0043] Furthermore, the organosilane is γ-methacryloxypropyltrimethoxysilane.

[0044] Furthermore, the stirring and mixing speed is 300-500 r / min, the stirring and mixing temperature is 100-150° C., and the stirring and mixing time is 3-10 min.

[0045] Furthermore, the temperature of the drying after mixing is 100-150° C., and the time of the drying after mixing is 2-3 hours.

[0046] Furthermore, during the process of mixing and drying the inorganic coated titanium dioxide and the organosilane, the inorganic nanoparticles on the surface of the inorganic coated titanium dioxide form a stable chemical bond with the organosilane.

[0047] Furthermore, the antioxidant in step 1 is a compound of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168) in a mass ratio of 1:2.

[0048] Furthermore, the lubricant in step 1 is one or more of silicone powder, pentaerythritol stearate and stearamide.

[0049] Furthermore, in step 1, the stirring temperature is 80-120° C., the stirring time is 1-3 min, and the stirring speed is 300-500 r / min.

[0050] Further, the processing temperature of the twin-screw extruder in the step 2 is 80-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 80-120°C, the second temperature zone is 250-270°C, the third temperature zone is 260-280°C, the fourth temperature zone is 260-280°C, the fifth temperature zone is 260-280°C, the sixth temperature zone is 250-270°C, the seventh temperature zone is 240-260°C, the eighth temperature zone is 240-260°C, the ninth temperature zone is 240-260°C, the tenth temperature zone is 240-260°C, the eleventh temperature zone is 250-270°C, and the twelfth temperature zone is 260-280°C.

[0051] Furthermore, the feeding rate of the twin-screw extruder in step 2 is 15-35 kg / h.

[0052] Furthermore, the screw speed of the twin-screw extruder in step 2 is 300-700 r / min.

[0053] Furthermore, the temperature of the extruder head of the twin-screw extruder in step 2 is 260-280°C.

[0054] Furthermore, the vacuum degree of the twin-screw extruder in step 2 is -0.08 to -0.09 MPa.

[0055] Furthermore, the torque of the twin-screw extruder in step 2 is 60-75 N·m.

[0056] Furthermore, the aspect ratio of the twin-screw extruder in step 2 is 52:1.

[0057] Furthermore, in step 3, the drying temperature is 80-120° C., and the drying time is 2-5 hours.

[0058] Furthermore, the injection temperature of the injection molding machine in step 3 is 250-310°C, divided into five temperature zones, wherein the first temperature zone is 250-260°C, the second temperature zone is 280-290°C, the third temperature zone is 300-310°C, the fourth temperature zone is 300-310°C, and the fifth temperature zone is 290-300°C.

[0059] Furthermore, the injection molding pressure of the injection molding machine in step 3 is 40-70 MPa.

[0060] Furthermore, the thickness of the modified polyphenylene ether in step 3 is 2-5 mm.

[0061] The present invention also provides a 5G base station material, and the 5G base station material is prepared from the modified polyphenylene ether. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 is a thermogravimetric analysis curve of the modified polyphenylene ether described in Example 1; Figure 2 This is the infrared spectrum of the modified polyphenylene ether described in Example 1.

[0063] Beneficial effects of the present invention: 1. The present invention uses polyphenylene ether as the main body, and adds polystyrene and toughening agent to modify it. The polyphenylene ether, polystyrene and toughening agent all contain double bond structures, which have better compatibility and also improve the impact resistance and tensile strength of polyphenylene ether. In addition, the present invention also adds modified titanium dioxide. Since titanium dioxide is an inorganic material and has poor compatibility with organic polymers, after organic treatment and inorganic coating, the compatibility between titanium dioxide and organic polymers is improved, and the dielectric loss of polyphenylene ether is reduced; 2. In the present invention, polyphenylene ether with low viscosity is used as raw material. If the viscosity of polyphenylene ether is too high, it will lead to poor processability, increased dielectric loss, poor dispersibility and poor modification effect after the subsequent addition of modified titanium dioxide. The polyphenylene ether in the present invention has low viscosity, good processability and good dispersibility of modified titanium dioxide. At the same time, the aspect ratio of the twin-screw extruder in the present invention is 52:1. Under this aspect ratio, the raw materials can fully react, and the titanium dioxide will not turn yellow due to long processing time. 3. The titanium dioxide used in the present invention is modified by compounding spherical titanium dioxide and rod-shaped titanium dioxide. The rod-shaped and spherical titanium dioxide are more evenly dispersed in the system due to their different shapes and can be filled into every corner of the organic polymer, so that the final modified polyphenylene ether has a higher dielectric constant and lower dielectric loss, and more stable performance. DETAILED DESCRIPTION

[0064] The invention is described in detail below with reference to the embodiments: The present invention provides a modified polyphenylene ether, a preparation method thereof and a 5G base station material. The mechanical properties of the material are improved by blending polyphenylene ether with polystyrene, and modified titanium dioxide is added to improve the dielectric constant of the material and reduce the dielectric loss of the material, thereby greatly improving its application range in the electrical field.

[0065] Example 1 The present embodiment provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 14g / 10min, and the heat deformation temperature of 0.45MPa is 173°C; the tensile strength of the modified polyphenylene ether is 65MPa, the flexural strength is 101MPa, and the 23°C simply supported beam notched impact strength is 6.5kJ / m 2The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5.4, and the dielectric loss at 23°C is 0.86*10 -3 .

[0066] In this embodiment, the polyphenylene ether is 33 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 15 parts by weight of spherical titanium dioxide and 36 parts by weight of rod-shaped titanium dioxide. The preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on a mixed titanium dioxide of 15 parts by weight of the quasi-spherical titanium dioxide and 36 parts by weight of the rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0067] This embodiment also provides a method for preparing modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0068] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0069] like Figure 1 This is a thermogravimetric analysis curve of the modified polyphenylene ether described in Example 1. It can be seen from the figure that the modified polyphenylene ether described in Example 1 starts to lose weight at an accelerated rate from 300°C, at which time polystyrene begins to decompose. At 330°C, the polyphenylene ether begins to decompose, and the weight loss rate accelerates. The weight loss temperature is above 300°C. The performance of the modified polyphenylene ether described in the present invention is stable.

[0070] like Figure 2 The infrared spectrum of the modified polyphenylene ether in Example 1 is shown in FIG. As can be seen from the figure, the modified polyphenylene ether in Example 1 has an infrared spectrum of 1181.15±0.01cm -1 The absorption peak of the CO bond of polyphenylene ether appears, 1377.61±0.01cm -1 The peak of the polyphenylene ether CH angle vibration absorption peak is 2918.25±0.01cm -1 It is the antisymmetric stretching vibration peak of -CH2 of polystyrene, 2850±0.01cm -1 It is the symmetrical stretching vibration peak of -CH2 of polystyrene.

[0071] Example 2 The present embodiment provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 11g / 10min, and the heat deformation temperature of 0.45MPa is 170°C; the tensile strength of the modified polyphenylene ether is 57MPa, the flexural strength is 92MPa, and the 23°C simply supported beam notched impact strength is 8kJ / m 2The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5.6, and the dielectric loss at 23°C is 0.87*10 -3 .

[0072] In this embodiment, the polyphenylene ether is 31 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 9 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 25 parts by weight of quasi-spherical titanium dioxide and 26 parts by weight of rod-shaped titanium dioxide. The preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on a mixed titanium dioxide of 25 parts by weight of the spherical titanium dioxide and 26 parts by weight of the rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0073] This embodiment also provides a method for preparing modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0074] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding amount of the twin-screw extruder is 25kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0075] Example 3 The present embodiment provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 15g / 10min, and the heat deformation temperature of 0.45MPa is 172°C; the tensile strength of the modified polyphenylene ether is 61MPa, the flexural strength is 97MPa, and the 23°C simply supported beam notched impact strength is 6kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5.9, and the dielectric loss at 23°C is 0.82*10 -3 .

[0076] In this embodiment, the polyphenylene ether is 33 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 25 parts by weight of quasi-spherical titanium dioxide and 26 parts by weight of rod-shaped titanium dioxide. The preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on a mixed titanium dioxide of 25 parts by weight of the spherical titanium dioxide and 26 parts by weight of the rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0077] This embodiment also provides a method for preparing modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0078] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 15kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0079] Example 4 The present embodiment provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 9.1g / 10min, and the heat deformation temperature of 0.45MPa is 175°C; the tensile strength of the modified polyphenylene ether is 65MPa, the flexural strength is 105MPa, and the 23°C simply supported beam notched impact strength is 7.6kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5.7, and the dielectric loss at 23°C is 0.9*10 -3 .

[0080] In this embodiment, the polyphenylene ether includes 18 parts by weight of polyphenylene ether with a viscosity of 0.35±0.02 dL / g at 25°C and a weight average molecular weight of 15000-25000, and 15 parts by weight of polyphenylene ether with a viscosity of 0.40±0.02 dL / g at 25°C and a weight average molecular weight of 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 25 parts by weight of quasi-spherical titanium dioxide and 26 parts by weight of rod-shaped titanium dioxide. The preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on a mixed titanium dioxide of 25 parts by weight of the spherical titanium dioxide and 26 parts by weight of the rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0081] This embodiment also provides a method for preparing modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0082] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0083] Comparative Example 1 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 12g / 10min, and the heat deformation temperature of 0.45MPa is 173°C; the tensile strength of the modified polyphenylene ether is 61MPa, the flexural strength is 102MPa, and the 23°C simply supported beam notched impact strength is 5.5kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 4.8, and the dielectric loss at 23°C is 0.8*10 -3 .

[0084] In this comparative example, the polyphenylene ether is 33 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 51 parts by weight of spherical titanium dioxide. The preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on 51 parts by weight of the quasi-spherical titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and after mixing, dried at 120° C. for 2 h to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0085] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0086] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0087] Comparative Example 2 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 12g / 10min, and the heat deformation temperature of 0.45MPa is 174°C; the tensile strength of the modified polyphenylene ether is 63MPa, the flexural strength is 104MPa, and the 23°C simply supported beam notched impact strength is 6kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 4.9, and the dielectric loss at 23°C is 0.79*10 -3 .

[0088] In this comparative example, the polyphenylene ether is 33 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 51 parts by weight of rod-shaped titanium dioxide, and the preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on 51 parts by weight of the rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0089] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0090] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0091] Comparative Example 3 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 7g / 10min, and the heat deformation temperature of 0.45MPa is 175°C; the tensile strength of the modified polyphenylene ether is 69MPa, the flexural strength is 109MPa, and the 23°C simply supported beam notched impact strength is 7.7kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 4.7, and the dielectric loss at 23°C is 0.85*10 -3 .

[0092] In this comparative example, the 18 parts by weight of polyphenylene ether having a viscosity of 0.35±0.02 dL / g at 25°C and a weight average molecular weight of 15000-25000, and the 15 parts by weight of polyphenylene ether having a viscosity of 0.40±0.02 dL / g at 25°C and a weight average molecular weight of 15000-25000; The polystyrene is 8 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 51 parts by weight of rod-shaped titanium dioxide, and the preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on 51 parts by weight of rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and after mixing, dried at 120° C. for 2 h to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0093] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0094] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0095] Comparative Example 4 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, modified titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 19g / 10min, and the heat deformation temperature of 0.45MPa is 163°C; the tensile strength of the modified polyphenylene ether is 63MPa, the flexural strength is 101MPa, and the 23°C simply supported beam notched impact strength is 7kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 4.3, and the dielectric loss at 23°C is 0.77*10 -3 .

[0096] In this comparative example, the polyphenylene ether is 36 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 12 parts by weight, and the melt index of the polystyrene at 200°C / 5kg is 4.5g / 10min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The modified titanium dioxide comprises 44 parts by weight of rod-shaped titanium dioxide, and the preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on 44 parts by weight of rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and then dried at 120° C. for 2 h after mixing to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0097] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0098] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0099] Comparative Example 5 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, modified titanium dioxide, antioxidant and lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 30g / 10min, and the heat deformation temperature of 0.45MPa is 148°C; the tensile strength of the modified polyphenylene ether is 55MPa, the flexural strength is 85MPa, and the 23°C simply supported beam notched impact strength is 8.1kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 3.5, and the dielectric loss at 23°C is 0.67*10 -3 .

[0100] In this comparative example, the polyphenylene ether is 36 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 27 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The modified titanium dioxide comprises 30 parts by weight of rod-shaped titanium dioxide, and the preparation process of the modified titanium dioxide is as follows: At room temperature, 6 parts by weight of aluminum oxide and 4 parts by weight of tin oxide are dispersed in 150 mL of deionized water to obtain an inorganic solution, and the inorganic solution is sprayed on 30 parts by weight of rod-shaped titanium dioxide under stirring at 300 r / min, and then rinsed with deionized water for 3 times, and dried at 100° C. for 2 h to obtain an inorganic coated titanium dioxide, and the inorganic coated titanium dioxide and 30 parts by weight of γ-methacryloxypropyltrimethoxysilane are stirred and mixed in a high mixing pot at 300 r / min and 100° C. for 5 min, and after mixing, dried at 120° C. for 2 h to obtain the modified titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0101] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0102] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0103] Comparative Example 6 The comparative example provides a modified polyphenylene ether, which is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, a toughening agent, titanium dioxide, an antioxidant and a lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 27g / 10min, and the heat deformation temperature of 0.45MPa is 150°C; the tensile strength of the modified polyphenylene ether is 56MPa, the flexural strength is 87MPa, and the 23°C simply supported beam notched impact strength is 8.6kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 4, and the dielectric loss at 23°C is 0.69*10 -3 .

[0104] In this comparative example, the polyphenylene ether is 36 parts by weight, the viscosity of the polyphenylene ether at 25° C. is 0.35±0.02 dL / g, and the weight average molecular weight is 15000-25000; The polystyrene is 27 parts by weight, and the melt index of the polystyrene at 200° C. / 5 kg is 4.5 g / 10 min; The toughening agent is 7 parts by weight of styrene-butadiene-styrene copolymer; The titanium dioxide comprises 30 parts by weight of spherical titanium dioxide; The antioxidant is 0.17 parts by weight of pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate and 0.33 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite; The lubricant is 0.5 parts by weight of pentaerythritol stearate.

[0105] This comparative example also provides a method for preparing a modified polyphenylene ether, which comprises weighing each component according to its content, and comprising the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, titanium dioxide, antioxidant and lubricant into a high-speed mixer, stirring for 1 minute at 100° C. and 350 r / min to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch at 100° C. for 4 hours, add the mixed masterbatch into an injection molding machine, and perform injection molding in the injection molding machine to obtain the modified polyphenylene ether of 2 mm.

[0106] The processing temperature of the twin-screw extruder is 120-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 120°C, the second temperature zone is 270°C, the third temperature zone is 280°C, the fourth temperature zone is 280°C, the fifth temperature zone is 280°C, the sixth temperature zone is 270°C, the seventh temperature zone is 260°C, the eighth temperature zone is 260°C, the ninth temperature zone is 260°C, the tenth temperature zone is 260°C, the eleventh temperature zone is 250°C, and the twelfth temperature zone is 260°C; the feeding rate of the twin-screw extruder is 35kg / h, the screw speed is 350r / min, the temperature of the extruder head is 280°C, the vacuum degree is -0.08MPa, the torque is 75N·m, and the aspect ratio is 52:1; The injection molding temperature of the injection molding machine is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250°C, the second temperature zone is 280°C, the third temperature zone is 300°C, the fourth temperature zone is 300°C, and the fifth temperature zone is 290°C; the injection molding pressure of the injection molding machine is 45MPa.

[0107] Table 1 shows the components and contents in Examples 1-4 and Comparative Examples 1-6

[0108] The antioxidant 1010 described in Table 1 is pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate, and the antioxidant 168 is tris(2,4-di-tert-butylphenyl) phosphite.

[0109] Table 2 shows the properties of the materials in Examples 1-4 and Comparative Examples 1-6

[0110] As shown in Tables 1 and 2, the modified polyphenylene ether in the present invention improves the dielectric constant of the material while ensuring the mechanical properties and processing properties of the material. At the same time, the dielectric loss will not increase significantly with the increase of the dielectric constant of the material, and the comprehensive performance of the material is strong. In Comparative Examples 1-4, a single titanium dioxide is used for mixing, resulting in the dielectric constant of the material failing to meet the requirements, and in Comparative Example 5, no toughening agent and polystyrene material are added, which significantly reduces the mechanical properties of the material. The titanium dioxide in Comparative Example 6 is not modified, and its mixing with the polyphenylene ether and polystyrene in the material is not complete, resulting in a lower dielectric constant of the material.

[0111] The test conditions of the modified polyphenylene ether in the present invention are as follows: the modified polyphenylene ether is allowed to stand at 23° C. for 24 hours before testing; Among them, the test standard for melt index is ISO 1133, the test standard for tensile strength is ISO 527, the test standard for flexural strength is ISO 178, the test standard for simply supported beam notched impact strength is ISO 179, and the test standard for dielectric constant and dielectric loss is GB / T 5594.4 2015.

[0112] Based on the above, it can be seen that the modified polyphenylene ether of the present invention has a wide range of applications, low cost and a very high market prospect.

[0113] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.

Claims

1. A modified polyphenylene ether, characterized in that: The modified polyphenylene ether is obtained by injection molding after blending and modifying polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant; the melt index of the modified polyphenylene ether at 300°C / 5kg is 9-15g / 10min, and the heat deformation temperature of 0.45MPa is 170-175°C; the tensile strength of the modified polyphenylene ether is 50-70MPa, the bending strength is 90-110MPa, and the 23°C simply supported beam notched impact strength is 6-8kJ / m 2 The dielectric constant of the modified polyphenylene ether at 1.1 GHz and 23°C is 5-7, and the dielectric loss at 23°C is (0.8-0.9)*10 -3 ; The components and contents in the modified polyphenylene ether are: Polyphenylene ether: 20-40 parts by weight; Polystyrene: 5-15 parts by weight; Toughening agent: 5-15 parts by weight; Modified titanium dioxide: 35-60 parts by weight; Antioxidant: 0.3-2 parts by weight; Lubricant: 0.3-2 parts by weight.

2. The modified polyphenylene ether according to claim 1, characterized in that: The polyphenylene ether has a viscosity of 0.35±0.02 dL / g and 0.4±0.02 dL / g at 25° C., or more than one of the above.

3. The modified polyphenylene ether according to claim 1, characterized in that: The toughening agent is styrene-butadiene-styrene copolymer.

4. The modified polyphenylene ether according to claim 1, characterized in that: The preparation process of the modified titanium dioxide is as follows: At room temperature, inorganic nanoparticles are dispersed in deionized water to obtain an inorganic solution, which is then sprayed onto titanium dioxide with stirring, and then rinsed with deionized water and dried to obtain an inorganic coated titanium dioxide. The inorganic coated titanium dioxide and organic silane are stirred and mixed in a high mixing pot, and then dried after mixing to obtain the modified titanium dioxide.

5. The modified polyphenylene ether according to claim 4, characterized in that: The titanium dioxide is rutile titanium dioxide, specifically including spherical titanium dioxide and rod-shaped titanium dioxide, and the mass ratio of the spherical titanium dioxide to the rod-shaped titanium dioxide is (1:1)-(1:2.4).

6. The modified polyphenylene ether according to claim 4, characterized in that: The organosilane is γ-methacryloxypropyltrimethoxysilane.

7. A method for preparing the modified polyphenylene ether according to any one of claims 1 to 6, characterized in that: Weigh each component according to its content, including the following steps: Step 1, putting polyphenylene ether, polystyrene, toughening agent, modified titanium dioxide, antioxidant and lubricant into a high-speed mixer and stirring to obtain a mixture; Step 2, placing the mixed material in the main feed port of a twin-screw extruder for extrusion, and cooling it with deionized water at room temperature to obtain a mixed masterbatch; Step 3: After drying the mixed masterbatch, add it into an injection molding machine for injection molding to obtain the modified polyphenylene ether.

8. The preparation method according to claim 7, characterized in that: The processing temperature of the twin-screw extruder in the step 2 is 80-280°C, which is divided into twelve temperature zones, wherein the first temperature zone is 80-120°C, the second temperature zone is 250-270°C, the third temperature zone is 260-280°C, the fourth temperature zone is 260-280°C, the fifth temperature zone is 260-280°C, the sixth temperature zone is 250-270°C, the seventh temperature zone is 240-260°C, the eighth temperature zone is 240-260°C, the ninth temperature zone is 240-260°C, the tenth temperature zone is 240-260°C, the eleventh temperature zone is 250-270°C, and the twelfth temperature zone is 260-280°C.

9. The preparation method according to claim 7, characterized in that: The injection temperature of the injection molding machine in step 3 is 250-310°C, which is divided into five temperature zones, wherein the first temperature zone is 250-260°C, the second temperature zone is 280-290°C, the third temperature zone is 300-310°C, the fourth temperature zone is 300-310°C, and the fifth temperature zone is 290-300°C.

10. A 5G base station material, characterized in that: The 5G base station material is prepared from the modified polyphenylene ether described in any one of claims 1-6.

Citation Information

Patent Citations

  • Low-dielectric-constant polyphenyl ether composition and preparation method thereof

    CN111393828A

Cited By

  • High-dielectric and low-loss material for antenna oscillator and preparation method of high-dielectric and low-loss material

    CN121517884A

  • Low-loss high-dielectric constant polyphenyl ether composite material and preparation method thereof

    CN121592156A