Biomass material composite intumescent flame retardant modified polyurethane foam material and preparation method thereof
By using modified insoluble dietary fiber as the carbon source of composite expansion-based flame retardant in polyurethane foam materials, the problems of flammability and poor flame retardant effects of polyurethane foam materials are solved, and high mechanical strength and stable flame retardant performance are achieved , while reducing the cost of material preparation and promoting the reuse of waste biomass materials.
Patent Information
- Application Number
- CN202411346223.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
Polyurethane foam materials are flammable and release toxic gases during combustion. The existing flame retardants have problems such as poor binding force, reduced mechanical properties and high cost, and the flame retardant effect is unstable.
Modified insoluble dietary fiber is used as the carbon source for the composite expansion-based flame retardant, and by combining with the physical, hydrogen and chemical bonds of the polyurethane matrix, a denser carbon layer is formed, which improves flame retardant performance and ensures mechanical strength.
It significantly improves the flame retardant properties and mechanical strength of polyurethane foam materials, reduces the cost of material preparation, realizes the reuse of waste biomass materials, and enhances the feasibility of industrial production.
Smart Images

Figure CN119060529A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane foam material, in particular to a biomass material composite expansion system flame retardant modified polyurethane foam material and a preparation method thereof, belonging to the technical field of polymer materials. Background Art
[0002] Polyurethane foam materials have the advantages of low density and thermal conductivity, high mechanical strength, and low cost. They are often used as thermal insulation materials in the fields of construction, transportation, and hot water pipes. However, since polyurethane materials contain a large number of combustible hydrocarbon segments and their porous structure makes the matrix have a large contact area with the air, they are extremely flammable, and the LOI value is only 17-19%, which poses a safety hazard. In addition, during the combustion process, toxic gases such as HCN, CO, NO, and NO2 are released, producing a large amount of thick smoke and droplets, which hinder the rescue of firefighters and seriously threaten the safety of people's lives and property.
[0003] At present, the flame retardant properties of polyurethane foam materials are often improved by adding flame retardant additives, which are divided into additive and reactive flame retardants according to the way they are added. Common additive flame retardants include metal oxides, phosphorus flame retardants, nitrogen flame retardants and expansion flame retardants; reactive flame retardants are modified by modifying their raw materials, such as flame retardant polyols and flame retardant isocyanates. However, additive flame retardants are mostly inorganic substances, which have poor bonding with the matrix. After addition, the mechanical properties of the material are reduced. They are easy to migrate out of the matrix during use, resulting in reduced flame retardant effect. Reactive flame retardants have unstable flame retardant effects, high costs, and are not suitable for large-scale production. They are currently in the exploratory stage.
[0004] Biomass flame retardants include cellulose, chitosan, lignin, starch and phytic acid, etc. They have a wide range of sources and are rich in carbon. During the thermal decomposition process, a carbon layer with heat insulation and oxygen isolation is formed on the surface of the matrix. It is a flame retardant with broad application prospects. However, due to its high C and H content, the flame retardant effect is poor when used. Summary of the invention
[0005] In order to solve the defects of the prior art, the first purpose of the present invention is to provide a biomass material composite intumescent flame retardant modified polyurethane foam material, which uses a composite intumescent flame retardant containing modified insoluble dietary fiber to modify the polyurethane foam material, thereby improving the flame retardant effect of the foam material while ensuring the high mechanical strength of the foam material.
[0006] The second object of the present invention is to provide a method for preparing a biomass material composite intumescent flame retardant modified polyurethane foam material, which has a wide source of raw materials, low cost, simple preparation method, and is conducive to industrial production.
[0007] In order to achieve the above technical objectives, the present invention provides a biomass material composite intumescent flame retardant modified polyurethane foam material, which is obtained by foaming and curing the following raw materials: the raw materials include a composite intumescent flame retardant, polyether polyol and / or polyester polyol, isocyanate, a catalyst, a foaming agent and a foam stabilizer; the composite intumescent flame retardant includes an acid source, a carbon source and a gas source; the acid source includes ammonium polyphosphate; the carbon source includes at least one of pentaerythritol, inositol, expandable graphite and modified insoluble dietary fiber; the gas source includes melamine; the modified insoluble dietary fiber includes at least one of ball-milled modified insoluble dietary fiber, oxidatively modified insoluble dietary fiber and silane coupling agent modified insoluble dietary fiber.
[0008] The key to the technical solution of the present invention is to use a small amount of modified insoluble dietary fiber as the carbon source in the composite intumescent flame retardant, and utilize the rich functional groups on the surface of these biomass materials to combine with the polyurethane matrix through physical, hydrogen bonds and chemical bonds, which is beneficial to enhance the bonding strength between the polyurethane matrix and the composite intumescent flame retardant, while better exerting the flame retardant effect of the composite intumescent flame retardant, ensuring the high mechanical strength of the foam material, and at the same time, the modified insoluble dietary fiber replaces part of the carbon source in the existing intumescent flame retardant, which is more conducive to quickly forming a denser and more stable carbon layer when encountering high temperature, thereby further improving the flame retardant performance of the material.
[0009] The modified insoluble dietary fiber of the present invention is selected from ball-milled modified insoluble dietary fiber, oxidatively modified insoluble dietary fiber and silane coupling agent modified insoluble dietary fiber. The insoluble dietary fiber is treated by mechanical ball milling or surface modification, which can reduce the size of the insoluble dietary fiber, enrich its surface functional groups, and facilitate its more uniform mixing in the polyurethane matrix material.
[0010] As a preferred solution, the raw materials include the following components by weight: 10 to 60 parts of composite intumescent flame retardant, 100 parts of polyether polyol and / or polyester polyol, 100 to 140 parts of isocyanate, 1 to 2 parts of catalyst, 10 to 30 parts of foaming agent, and 1 to 3 parts of foam stabilizer. The composite intumescent flame retardant is preferably 15 to 35 parts by weight.
[0011] As a more preferred solution, the composite intumescent flame retardant is composed of an acid source, a carbon source and a gas source in a mass ratio of 3:0.5-1.5:0.5-1.5; the mass proportion of the modified insoluble dietary fiber in the carbon source is 40-60%.
[0012] The insoluble dietary fiber involved in the present invention is obtained by extracting bean dregs by enzyme-alkali method. The enzyme-alkali method is a conventional method in the prior art, and neutral protease and alkaline solution are used to treat the bean dregs to extract insoluble dietary fiber. The specific process of extracting insoluble dietary fiber from bean dregs by enzyme-alkali method is as follows: using bean dregs as raw materials, washing the bean dregs with deionized water, and placing them in an 80°C forced air drying oven for drying until the moisture in the bean dregs is removed. The dried bean dregs are crushed and passed through a 100-mesh sieve, and an appropriate amount of sieved bean dregs powder is weighed as a raw material, the amount of neutral protease added is 0.2% of the mass of the bean dregs, the alkali solution is 4wt% of Na2CO3 solution, the ratio of bean dregs powder to alkali solution is 1 (w): 20 (v), the extraction time is 50min, the extraction temperature is 70°C, and after the leaching is completed, the above suspension is filtered, the alkali solution in the filter residue is washed with deionized water, and the insoluble dietary fiber is obtained after drying.
[0013] As a preferred solution, the ball-milled modified insoluble dietary fiber is obtained by activating the insoluble dietary fiber through ball milling. After the insoluble dietary fiber is ball milled, its dispersibility is better, and its size is refined, so that it can be more evenly dispersed in the polyurethane matrix.
[0014] As a preferred solution, the oxidatively modified insoluble dietary fiber is obtained by oxidizing the insoluble dietary fiber. The oxidatively modified insoluble dietary fiber is obtained by further oxidizing the insoluble dietary fiber. The insoluble dietary fiber is oxidized for 2 hours in a 100°C water bath in a 2wt% to 5wt% hydrogen peroxide solution. In order to allow the biomass material to fully contact the oxidant, stirring is used during the oxidation process. After the oxidation is completed, the oxidatively modified insoluble dietary fiber is obtained by filtering and drying. After the insoluble dietary fiber is oxidized, the active groups on its surface will increase, and the reaction activity will be stronger.
[0015] As a preferred solution, the silane coupling agent modified insoluble dietary fiber is obtained by modifying insoluble dietary fiber with a silane coupling agent. The silane coupling agent modified insoluble dietary fiber is obtained by further surface treating the insoluble dietary fiber with a silane coupling agent solution to enhance the interfacial bonding between it and the polymer matrix, and ultrasonically treating it to enhance dispersibility for 30 minutes, and then stirring it in a 100°C water bath for 2 hours. After the treatment is completed, the suspension is centrifuged, and the filter residue obtained by filtration is the silane coupling agent modified insoluble dietary fiber. The silane coupling agent includes KH550 and / or KH560. After the insoluble dietary fiber is modified with a silane coupling agent, its compatibility with the polyurethane matrix is significantly improved.
[0016] As a preferred solution, the isocyanate includes polymethylene polyphenyl polyisocyanate and / or diphenylmethane diisocyanate.
[0017] As a preferred solution, the catalyst includes triethylenediamine and / or pentamethyldiethylenetriamine.
[0018] As a preferred solution, the foaming agent includes sodium dodecyl sulfate. Using sodium dodecyl sulfate instead of deionized water as a surface modifier is helpful for preparing high-strength polyurethane foam materials. Using sodium dodecyl sulfate instead of deionized water as a foaming agent is helpful for obtaining high-strength polyurethane foam materials.
[0019] As a preferred solution, the foam stabilizer includes silicone oil.
[0020] The present invention also provides a method for preparing a biomass material composite expansion flame retardant modified polyurethane foam material, which comprises uniformly mixing polyether polyol, composite expansion flame retardant and auxiliary agents including catalyst, foaming agent and foam stabilizer, slowly adding isocyanate, and vigorously stirring for foaming and curing to obtain the foam material.
[0021] As a preferred solution, the foaming time is 10 to 20 seconds.
[0022] As a preferred solution, the curing temperature is 80-100° C. and the curing time is 8h-12h.
[0023] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0024] The modified insoluble dietary fiber of the technical solution of the present invention is derived from waste biomass materials, which realizes the reuse of waste agricultural and sideline products and is beneficial to preventing their damage to the environment. From an economic point of view, biomass materials are cheaper than traditional carbon sources, which is beneficial to reducing the preparation cost of materials.
[0025] The composite intumescent flame retardant obtained by introducing modified insoluble dietary fiber in the technical solution of the present invention can enhance its dispersibility and stability in the polyurethane group, which is beneficial to enhancing the bonding strength between the polyurethane matrix and the composite intumescent flame retardant, while better exerting the flame retardant effect of the composite intumescent flame retardant and ensuring the high mechanical strength of the foam material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the polyurethane rigid foam prepared in Example 1 of the present invention.
[0027] Figure 2 This is a diagram of the compression resistance of polyurethane rigid foams with different flame retardant contents prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0029] In the following specific embodiment, the specific process of extracting insoluble dietary fiber from bean dregs by enzyme-alkali method is as follows: bean dregs are used as raw materials, after washing the bean dregs with deionized water, they are placed in an 80°C forced air drying oven for drying until the moisture in the bean dregs is removed. The dried bean dregs are crushed and passed through a 100-mesh sieve, and an appropriate amount of bean dregs powder after sieving is weighed as a raw material, the amount of neutral protease added is 0.2% of the mass of the bean dregs, the alkali solution is a 4wt% Na2CO3 solution, the ratio of bean dregs powder to alkali solution is 1(w):20(v), the extraction time is 50min, the extraction temperature is 70°C, and after leaching, the above suspension is filtered, the alkali solution in the filter residue is washed with deionized water, and the insoluble dietary fiber is obtained after drying.
[0030] Example 1
[0031] 1. Oxidative modification of insoluble dietary fiber:
[0032] After physically grinding the insoluble dietary fiber, a 4wt% hydrogen peroxide solution is used to modify the surface of the insoluble dietary fiber, wherein the treatment temperature is 90°C and the treatment time is 2h. After the oxidation treatment is completed, the suspension is filtered and the filter residue is dried to obtain oxidatively modified insoluble dietary fiber.
[0033] 2. Preparation of polyurethane rigid foam:
[0034] Polyurethane rigid foam was prepared by a one-step foaming method. The dosage of polyether polyol (polyether polyol 4110 produced by Yihuiyang New Materials Co., Ltd.) and polymethylene polyphenyl polyisocyanate (PM200, produced by Yihuiyang New Materials Co., Ltd.) was 1:1, both of which were 36 g. The content of sodium dodecyl sulfonate (foaming agent) was 7 g, the content of triethylenediamine (catalyst) was 0.7 g, and the content of silicone oil (foam stabilizer) was 0.7 g. The total content of flame retardant was controlled to be 20% (accounting for the total mass of polyether polyol and isocyanate), of which the content of ammonium polyphosphate (acid source) in the flame retardant was 8.64 g, the content of melamine (gas source) was 2.88 g, the content of inositol (carbon source) was 1.44 g, and the content of oxidatively modified insoluble dietary fiber (carbon source) was 1.44 g. During the preparation process, the polyether polyol, flame retardant and additives are first mixed evenly, and then the isocyanate is slowly added and vigorously stirred for 10 to 20 seconds to obtain polyurethane rigid foam. The compression resistance is tested, and the combustion performance is tested according to the GBT2408-2021 standard. The compression resistance of the polyurethane rigid foam reaches 38.1MPa, and the vertical combustion performance is changed from the V-2 level before modification to the V-0 level.
[0035] Example 2
[0036] The difference from Example 1 is that the total content of the flame retardant is controlled to be 5%, 10%, 15%, and 25% (accounting for the total mass of the polyether polyol and the isocyanate), and the 20% in Example 1 is used as a control, wherein the mass ratio of the acid source, melamine, inositol, and oxidatively modified insoluble dietary fiber in the flame retardant is kept unchanged at 3:1:0.5:0.5. Figure 2 ,With the increasing proportion of flame retardant, its mechanical properties show a downward trend, but the compressive strength remains above 37.5MPa.
[0037] Example 3
[0038] 1. Extraction of insoluble dietary fiber and modification with silane coupling agent:
[0039] After physically grinding the insoluble dietary fiber, a 5wt% silane coupling agent KH550 solution is used to modify the surface of the insoluble dietary fiber, wherein the treatment temperature is 90°C and the treatment time is 2h. During the treatment process, mechanical stirring is used to make the silane coupling and the insoluble dietary fiber contact more fully. After the treatment is completed, the filter is filtered and the filter residue is dried to obtain the silane coupling agent modified insoluble dietary fiber.
[0040] 2. Silane coupling agent modified insoluble dietary fiber synergistic expansion flame retardant modified polyurethane rigid foam:
[0041] Polyurethane rigid foam was prepared by a one-step foaming method. The dosage of polyether polyol (polyether polyol 4110 produced by Yihuiyang New Materials Co., Ltd.) and polymethylene polyphenyl polyisocyanate (PM200, produced by Yihuiyang New Materials Co., Ltd.) was 1:1, both were 36 g, the content of sodium dodecyl sulfonate (foaming agent) was 7 g, the content of triethylenediamine (catalyst) was 0.7 g, the content of silicone oil (foam stabilizer) was 0.7 g, and the total content of flame retardant was controlled to be 20% (accounting for the total mass of polyether polyol and isocyanate), of which the content of ammonium polyphosphate (acid source) in the flame retardant was 8.64 g, the content of melamine (gas source) was 2.88 g, the content of inositol (carbon source) was 1.44 g, and the content of silane-modified insoluble dietary fiber (carbon source) was 1.44 g. During the preparation process, the polyether polyol, flame retardant and additives are first mixed evenly, and then the isocyanate is slowly added and stirred vigorously for 10 to 20 seconds to obtain polyurethane rigid foam. The compression resistance is tested, and the combustion performance is tested according to the GBT2408-2021 standard. The compression resistance of the polyurethane rigid foam reaches 38.5MPa, and the vertical combustion performance is changed from the V-2 level before modification to the V-0 level.
[0042] Comparative Example 1
[0043] Comparative experiment: Compare the effects of adding unmodified insoluble dietary fiber on the mechanical properties and flame retardant properties of composite materials.
[0044] Compared with Example 1, the only difference is that insoluble dietary fiber is used. The compression resistance is tested, and the combustion performance is tested according to the GBT2408-2021 standard. The compression resistance of the polyurethane rigid foam is 36.5 MPa, and the vertical combustion performance is changed from the V-2 level before modification to the V-0 level.
[0045] The unmodified insoluble dietary fiber added to the polyurethane foam material has a poorer bonding effect with the matrix than the modified one, and defects such as voids and gaps appear. Although the vertical combustion performance reaches the V-0 level, the flame combustion time is longer than that after modification, and the flame retardant performance is slightly reduced. The first flame combustion time of the material increases from 2.1s to 4.3s, and the second flame combustion time increases from 0.9s to 1.8s.
Claims
1. A biomass material composite intumescent flame retardant modified polyurethane foam material, characterized in that: Obtained by foaming and curing the following raw materials: The raw materials include composite expansion flame retardant, polyether polyol and / or polyester polyol, isocyanate, catalyst, foaming agent and foam stabilizer; The composite intumescent flame retardant comprises an acid source, a carbon source and a gas source; The acid source includes ammonium polyphosphate; The carbon source comprises at least one of pentaerythritol, inositol, expandable graphite and modified insoluble dietary fiber; The gas source includes melamine; The modified insoluble dietary fiber includes at least one of ball-milled modified insoluble dietary fiber, oxidatively modified insoluble dietary fiber and silane coupling agent modified insoluble dietary fiber.
2. The biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 1, characterized in that: The raw materials include the following components by weight: 10-60 parts of composite expansion flame retardant, 100 parts of polyether polyol and / or polyester polyol, 100-140 parts of isocyanate, 1-2 parts of catalyst, 10-30 parts of foaming agent and 1-3 parts of foam stabilizer.
3. The biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 2, characterized in that: The composite intumescent flame retardant is composed of an acid source, a carbon source and a gas source in a mass ratio of 3:0.5-1.5:0.5-1.5; The mass proportion of the modified insoluble dietary fiber in the carbon source is 40-60%.
4. A biomass material composite intumescent flame retardant modified polyurethane foam material according to any one of claims 1 to 3, characterized in that: The oxidatively modified insoluble dietary fiber is obtained by subjecting the insoluble dietary fiber to an oxidative treatment; The ball-milled modified insoluble dietary fiber is obtained by activating the insoluble dietary fiber through ball milling; The silane coupling agent modified insoluble dietary fiber is obtained by modifying insoluble dietary fiber with a silane coupling agent.
5. A biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 1 or 2, characterized in that: The isocyanate includes polymethylene polyphenyl polyisocyanate and / or diphenylmethane diisocyanate.
6. A biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 1 or 2, characterized in that: The catalyst includes triethylenediamine and / or pentamethyldiethylenetriamine.
7. A biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 1 or 2, characterized in that: The foaming agent includes sodium dodecyl sulfonate; The foam stabilizer includes silicone oil.
8. The method for preparing a biomass material composite intumescent flame retardant modified polyurethane foam material according to any one of claims 1 to 7, characterized in that: The polyether polyol and / or polyester polyol, composite expansion flame retardant and auxiliary agents including catalyst, foaming agent and foam stabilizer are uniformly mixed, and then isocyanate is slowly added, and the mixture is vigorously stirred for foaming and curing to obtain the product.
9. The method for preparing a biomass material composite intumescent flame retardant modified polyurethane foam material according to claim 8, characterized in that: The foaming time is 10 to 20 seconds.