Self-lubricating wear-resistant polyphenylene sulfide-based composite material and preparation method thereof

By modifying polydopamine on the surface of polyphenylene sulfide particles and coating benzimidazole fluorinated polyimide gel to form interface modified polyphenylene sulfide particles, the performance of polyphenylene sulfide materials in the field of high wear resistance is solved. The best problem has achieved the improvement of the wear resistance and mechanical strength of the material.

CN119060537AActive Publication Date: 2024-12-03JIANGXI JUZHEN TECH DEV CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411320509.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Existing polyphenylene sulfide materials have poor performance in the field of high wear resistance, insufficient friction coefficient and mechanical strength, and cannot meet certain application needs.

Method used

Polydopamine is modified on the surface of polyphenylene sulfide particles to form polyphenylene sulfide@polydopamine microspheres, and coated with benzimidazole fluorinated polyimide gel and then freeze-dried to form a composite phase interface to form an interface modification to form an interface The polyphenylene sulfide particles are then combined with other reinforcing materials to form a self-lubricated wear-resistant polyphenylene sulfide-based composite material.

Benefits of technology

On the basis of maintaining a low coefficient of friction, the material's wear resistance and mechanical strength are significantly improved, and the application needs of high wear resistance and high strength are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005053734610000081
    Figure BDA0005053734610000081
  • Figure BDA0005053734610000091
    Figure BDA0005053734610000091
Patent Text Reader

Abstract

The invention relates to a self-lubricating wear-resistant polyphenylene sulfide-based composite material which comprises the following raw materials in parts by mass: 75-90 parts of interface modified polyphenylene sulfide particles, 5-10 parts of polytetrafluoroethylene particles, 10-20 parts of reinforced fibers and 0.2-1 part of a lubricant, the interface modified polyphenylene sulfide particles are prepared by the following steps: polymerizing dopamine on the surfaces of polyphenylene sulfide particles to form polyphenylene sulfide and polydopamine (PPS and PDA) microspheres, coating benzimidazole fluorinated polyimide gel, and freeze-drying to form a composite phase interface. The dosage of the dopamine is 1-3 wt% of the polyphenylene sulfide particles; the dosage of the benzimidazole fluorinated polyimide gel is 20 to 30 weight percent of that of the PPS (at) PDA microspheres. The polyphenylene sulfide-based composite material prepared by the invention has excellent wear resistance and mechanical strength on the basis of maintaining a relatively low friction coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a self-lubricating and wear-resistant polyphenylene sulfide-based composite material and a preparation method thereof. Background Art

[0002] Polyphenylene sulfide (PPS) is a semi-crystalline engineering plastic with excellent comprehensive performance. It has excellent thermal stability, flame retardancy, chemical stability and corrosion resistance, and has high hardness and strength. Therefore, it is widely used in aerospace, military equipment and automobile manufacturing. However, pure PPS is brittle and has poor wear resistance. It cannot meet the application requirements in areas that require high wear resistance. It must be modified or reinforced materials must be added to improve its friction and wear performance. Generally, the friction and wear performance of PPS is improved by adding fillers such as fibers and solid lubricants or liquid lubricants, but it still cannot meet the wear resistance requirements in many fields such as bearings, bushings or gears. Therefore, the use of self-lubricating and wear-resistant PPS modified materials with excellent performance as equipment parts has great practical significance and value.

[0003] CN115785671A discloses an aerogel / polyphenylene sulfide self-lubricating friction material, which is a mixture of polyphenylene sulfide, aerogel, reinforcing fiber and liquid phase auxiliary agent, melt extruded to obtain an aerogel / polyphenylene sulfide self-lubricating friction material. The polyphenylene sulfide material is modified by low thermal conductivity, high porosity aerogel and reinforcing fiber, which greatly reduces the friction coefficient of the material. However, by melt blending, the PPS matrix and aerogel are evenly dispersed, which is essentially still a physical blending modification method. The stability of the system is not good enough, and it is easy to produce migration, agglomeration and other phenomena, resulting in poor wear resistance of the material.

[0004] The inventor disclosed a low friction coefficient polyphenylene sulfide material in the previous patent CN 116925547 B. The polyphenylene sulfide powder particle microstructure is coated with a layer of polymer aerogel to form a composite phase interface, and then melt-compounded with other components to form a polyphenylene sulfide composite material. When friction occurs with other materials, the composite phase interface on the polyphenylene sulfide microstructure can block or reduce the heat generated by friction and transfer to the polyphenylene sulfide material, thereby reducing the occurrence of material creep. At the same time, the composite phase interface on the polyphenylene sulfide microstructure can reduce the generation of friction, thereby reducing the material friction coefficient and improving wear resistance. In fact, the surface of the polyphenylene sulfide powder particle is coated with a polyimide gel containing metal sulfide and polar solvent, and then heat-treated in a vacuum oven, the polyimide gel is converted into aerogel, and the interface-modified polyphenylene sulfide powder particles are obtained. During the vacuum oven treatment, metal sulfide can react with the Cl bond remaining at the end of the polyphenylene sulfide molecular chain, and may also react with the carboxyl group at the end of the polyimide polymer in the polyimide gel, so that the polyimide gel has a strong adhesion to the surface of the polyphenylene sulfide particles. The polar solvent in the polyimide gel will gradually evaporate during the heating process to form a polyimide aerogel, forming a solid-gas composite phase interface at the polyphenylene sulfide interface. The friction coefficient of the polyphenylene sulfide material after interface modification is reduced, but the wear resistance and mechanical strength need to be improved. Summary of the invention

[0005] In view of the problem that the wear resistance and mechanical strength of polyphenylene sulfide in the above-mentioned prior art are still unsatisfactory, the present invention provides a self-lubricating wear-resistant polyphenylene sulfide-based composite material and a preparation method thereof. The present invention first modifies the surface of polyphenylene sulfide particles with polydopamine to form polyphenylene sulfide@polydopamine microspheres, then coats the surface of the microspheres with benzimidazole fluorinated polyimide gel and freeze-dries to form a composite phase interface to obtain interface-modified polyphenylene sulfide particles; finally, the polyphenylene sulfide-based composite material formed by compounding the interface-modified polyphenylene sulfide particles with other reinforcing materials has excellent wear resistance and mechanical strength while maintaining a low friction coefficient.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A self-lubricating and wear-resistant polyphenylene sulfide-based composite material comprises the following raw materials in parts by weight: 75-90 parts of interface-modified polyphenylene sulfide particles, 5-10 parts of polytetrafluoroethylene particles, 10-20 parts of reinforcing fibers, and 0.2-1 parts of lubricants; the interface-modified polyphenylene sulfide particles are obtained by polymerizing dopamine on the surface of polyphenylene sulfide particles to form polyphenylene sulfide@polydopamine (PPS@PDA) microspheres, coating benzimidazole fluorinated polyimide gel, and then freeze-drying to form a composite phase interface; the amount of dopamine used is 1-3wt% of the polyphenylene sulfide particles; the amount of benzimidazole fluorinated polyimide gel used is 20-30wt% of the PPS@PDA microspheres.

[0008] Furthermore, the dosage of dopamine is 2-3wt% of the polyphenylene sulfide particles; the dosage of benzimidazole fluorinated polyimide gel is 25-30wt% of the PPS@PDA microspheres.

[0009] Furthermore, the benzimidazole fluorinated polyimide gel is obtained by reacting fluorinated dianhydride, benzimidazole diamine and 1,3,5-benzenetricarboxylic acid chloride to obtain benzimidazole fluorinated polyamic acid, which is then imidized; the molar ratio of the fluorinated dianhydride, benzimidazole diamine and 1,3,5-benzenetricarboxylic acid chloride is 1: (1.05-1.15): (0.01-0.02); the reaction is carried out in a polar organic solvent, and the polar organic solvent accounts for 55-70wt%.

[0010] Furthermore, the fluorinated dianhydride is selected from at least one of 4,4'-hexafluoroisopropylidenephthalic anhydride (6FDA) and 4,4'-[2,2,2-trifluoro-1-(3-trifluoromethyl-phenyl)ethylidene]diphthalic anhydride (TFDA);

[0011] The benzimidazole diamine is selected from at least one of benzimidazole-1,2-diamine, 1H-benzo[D]imidazole-5,6-diamine, 1H-benzo[D]imidazole-2,5-diamine, 1H-benzo[D]imidazole-2,7-diamine, and 5,6-dimethyl-1H-benzo[D]imidazole-4,7-diamine; and the polar organic solvent is at least one of N,N′-dimethylacetamide (DMAC), N,N′-dimethylformamide (DMF), and N-methylpyrrolidone (NMP).

[0012] Furthermore, the benzimidazole fluorinated polyimide gel is prepared by a preparation method comprising the following steps:

[0013] (P1) Under an inert atmosphere, a benzimidazole diamine is dissolved in a polar organic solvent, and a fluorinated dianhydride is added to carry out a pre-condensation reaction at 5 to 10° C. for 4 to 6 hours, and then 1,3,5-benzenetricarboxylic acid chloride is added to continue the reaction for 0.5 to 1 hour to obtain a benzimidazole fluorinated polyamic acid solution;

[0014] (P2) adding a water-carrying agent to a benzimidazole fluorinated polyamic acid solution, heating to 180-220° C. to carry out an imide condensation reaction until no water is discharged, cooling to room temperature and aging to obtain a benzimidazole fluorinated polyimide gel.

[0015] Furthermore, the inert atmosphere in step (P1) is at least one of nitrogen or argon.

[0016] Furthermore, in step (P2), the water-carrying agent is at least one of toluene and xylene, and the amount of the water-carrying agent is 0.8 to 1.2 times the mass of the organic polar solvent; and the aging time is 3 to 5 days.

[0017] Furthermore, the number average molecular weight of the polyphenylene sulfide is 30,000 to 50,000.

[0018] Furthermore, the interface-modified polyphenylene sulfide particles are prepared by a preparation method comprising the following steps:

[0019] (S1) adding polyphenylene sulfide particles and dopamine into a Tris-HCl buffer solution, stirring and reacting at 20-30° C. for 4-8 hours, and after the reaction is completed, centrifuging, washing, and drying to obtain polydopamine-modified polyphenylene sulfide particles, namely, PPS@PDA microspheres;

[0020] (S2) PPS@PDA microspheres and benzimidazole fluorinated polyimide gel are stirred and mixed in a rolling ball machine so that the surface of the PPS@PDA microspheres is coated with a layer of benzimidazole fluorinated polyimide gel; and then the microspheres are freeze-dried so that the benzimidazole fluorinated polyimide gel is converted into aerogel and coated on the surface of the PPS@PDA microspheres, thereby obtaining interface-modified polyphenylene sulfide particles.

[0021] Furthermore, in step (S1), the concentration of the Tris-HCl buffer solution is 10-30 mM, and the pH is 8.0-9.0; the volume ratio of the mass of the dopamine to the Tris-HCl buffer solution is 1-3 g: 1000 mL; and the drying is performed in a vacuum oven at 60-80° C. for 12-24 hours. Steps The stirring reaction time in step (S1) needs to be controlled within an appropriate range. If the stirring reaction time is too short, the modification amount of polydopamine is too low, and the effect is limited; if the stirring reaction time is too long, the modification amount is too high, and the PPS@PDA microspheres are prone to adhesion.

[0022] Furthermore, in step (S2), the stirring and mixing conditions are: a ball rolling machine speed of 100 to 200 rpm, and a time of 1 to 2 hours; the freeze-drying conditions are: first freezing in liquid nitrogen for 0.5 to 1 hour, and then vacuum drying in a cold trap at -50 to -40°C for 24 to 48 hours, and a vacuum degree of 10 to 30 Pa.

[0023] Furthermore, the particle size of the interface modified polyphenylene sulfide particles is 10 to 60 μm, and the particle size of the polytetrafluoroethylene particles is 5 to 15 μm.

[0024] Furthermore, the reinforcing fiber is at least one of glass fiber, carbon fiber, chopped aramid fiber, and basalt fiber; the reinforcing fiber has a diameter of 2 to 10 μm and a length of 1 to 3 mm.

[0025] Furthermore, the lubricant is at least one of amino silicone oil, methyl silicone oil, ethyl silicone oil, and polyether modified silicone oil.

[0026] In a second aspect, the present invention also provides a method for preparing the above-mentioned wear-resistant self-lubricating polyphenylene sulfide-based composite material, comprising the following steps: mixing interface-modified polyphenylene sulfide particles with polytetrafluoroethylene particles, reinforcing fibers, and a lubricant, and then mixing and extruding to obtain a wear-resistant self-lubricating polyphenylene sulfide-based composite material.

[0027] Furthermore, the mixing and extruding is carried out in a twin-screw extruder at an extrusion temperature of 280-320° C.; and granulation is also included after the mixing and extruding.

[0028] The invention firstly adopts dopamine to undergo a self-polymerization oxidation reaction under alkaline conditions, and modifies the surface of polyphenylene sulfide particles with polydopamine to form PPS@PDA microspheres; then, a fluorinated dibasic anhydride, a benzimidazole diamine and a cross-linking agent 1,3,5-benzenetricarboxylic acid chloride are reacted to prepare a benzimidazole fluorinated polyimide gel, which is coated on the surface of the PPS@PDA microspheres and then freeze-dried to form a composite phase interface; during the freeze-drying process, the organic polar solvent in the benzimidazole fluorinated polyimide gel slowly evaporates, and the gel is gradually transformed into an aerogel coated on the surface of the PPS@PDA microspheres. Compared with conventional polyimide aerogels, the introduction of benzimidazole fluorinated polyimide aerogels significantly improves the wear resistance of polyphenylene sulfide particles. The possible reason is that the introduction of benzimidazole heterocycles and fluorine atoms in imidazole fluorinated polyimide brings about the improvement of wear resistance; at the same time, the introduction of cross-linking agent 1,3,5-benzenetricarboxylic acid chloride increases the density of imidazole fluorinated polyimide. In addition, polydopamine on PPS@PDA microspheres has strong adhesion, thereby enhancing the interfacial force between polyphenylene sulfide particles and benzimidazole fluorinated polyimide aerogels; on the other hand, the hydroxyl groups in polydopamine can react with the terminal amino groups in imidazole fluorinated polyimide, further increasing the density of benzimidazole fluorinated polyimide, thereby improving the mechanical strength and wear resistance of the interface-modified polyphenylene sulfide particles. In summary, the polyphenylene sulfide-based composite materials formed by the interface-modified polyphenylene sulfide particles modified by polydopamine and coated by benzimidazole fluorinated polyimide aerogel and compounded with other reinforcing materials have good wear resistance and low friction coefficient.

[0029] The present invention forms interface-modified polyphenylene sulfide particles by polydopamine modification and coating of benzimidazole fluorinated polyimide aerogel, and the polyphenylene sulfide-based composite material formed by compounding the particles with other reinforcing materials has excellent wear resistance and mechanical strength while maintaining a low friction coefficient. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents in the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by mass. Unless otherwise specified, the reagents used are all commercially available reagents in this area.

[0031] Polyphenylene sulfide particles, with a number average molecular weight of about 42,000 and a particle size of about 30 μm, were selected from Chongqing Jushi New Material Technology Co., Ltd.;

[0032] Polytetrafluoroethylene particles, with a particle size of about 8 μm, were selected from Zhejiang Ge Rui New Materials Co., Ltd.;

[0033] Glass fiber, about 8 μm in diameter and about 2 mm in length, selected from China Jushi Co., Ltd.;

[0034] Dopamine and Tris-HCl buffer solution were selected from Aladdin Reagent Company.

[0035] Preparation of benzimidazole fluorinated polyimide gel

[0036] Preparation Example 1

[0037] (P1) A three-necked flask was equipped with a stirrer and a reflux cooling air pipe, and then 155.6 g (1.05 mol) of 1H-benzo[D]imidazole-5,6-diamine and 1000 g of N,N′-dimethylacetamide (DMAC) were added thereto, and stirred for 30 min under nitrogen flow to completely dissolve them; then 444.2 g (1 mol) of 4,4′-hexafluoroisopropylidenephthalic anhydride (6FDA) was added to carry out a pre-condensation reaction at 6±1° C. for 6 h; and then 2.66 g (0.01 mol) of 1,3,5-benzenetricarboxylic acid chloride was added to continue the reaction for 0.5 h to obtain a benzimidazole fluorinated polyamic acid solution;

[0038] (P2) 800 g of toluene is added as a water-carrying agent to the above-mentioned benzimidazole-based fluorinated polyamic acid solution, and the solution is heated to 200° C. to carry out an imide condensation reaction until no water is discharged. The solution is cooled to room temperature and aged for 3 days to obtain a benzimidazole-based fluorinated polyimide gel a.

[0039] Preparation Example 2

[0040] (P1) A three-necked flask was equipped with a stirrer and a reflux cooling air pipe, and then 170.4 g (1.15 mol) of benzimidazole-1,2-diamine and 1000 g of N,N′-dimethylacetamide (DMAC) were added thereto, and stirred for 30 min under nitrogen flow to completely dissolve them; then 444.2 g (1 mol) of 4,4′-hexafluoroisopropylidenephthalic anhydride (6FDA) was added and pre-polycondensed at 8±1° C. for 4 h; then 5.32 g (0.02 mol) of 1,3,5-benzenetricarboxylic acid chloride was added and the reaction was continued for 0.5 h to obtain a benzimidazole fluorinated polyamic acid solution;

[0041] (P2) 800 g of toluene was added as a water-carrying agent to the above-mentioned benzimidazole fluorinated polyamic acid solution, and the solution was heated to 210° C. to carry out an imide condensation reaction until no water was discharged. The solution was cooled to room temperature and aged for 3 days to obtain a benzimidazole fluorinated polyimide gel b.

[0042] Comparative Preparation Example 1

[0043] (P1) A three-necked flask was equipped with a stirrer and a reflux cooling air pipe, and then 210.2 g (1.05 mol) of 4,4′-diaminodiphenyl ether (ODA) and 1000 g of N,N′-dimethylacetamide (DMAC) were added thereto, and stirred for 30 min under nitrogen flow to completely dissolve them; then 294.2 g (1 mol) of 3,3′,4,4′-biphenyltetracarboxylic dianhydride (BPDA) was added and pre-polycondensed at 6±1° C. for 6 h; then 2.66 g (0.01 mol) of 1,3,5-benzenetricarboxylic acid chloride was added and the reaction was continued for 0.5 h to obtain a polyamic acid solution;

[0044] (P2) 800 g of toluene was added as a water-carrying agent to the polyamic acid solution, and the solution was heated to 200° C. to carry out an imide condensation reaction until no water was discharged. The solution was cooled to room temperature and aged for 3 days to obtain a polyimide gel.

[0045] Example 1

[0046] (S1) 100 g of polyphenylene sulfide particles and 1 g of dopamine were added to 1000 mL of Tris-HCl buffer solution (Ph=8.0, 10 mM), and stirred at 20° C. for 6 h. After the reaction was completed, the polydopamine-modified polyphenylene sulfide particles, i.e., PPS@PDA microspheres, were obtained after centrifugation, washing, and drying at 80° C. for 12 h.

[0047] (S2) 100 parts of PPS@PDA microspheres and 20 parts of the benzimidazole fluorinated polyimide gel a prepared in Preparation Example 1 were subjected to a rolling process at 150 rpm for 1 h, so that the surface of the PPS@PDA microspheres was coated with a layer of the benzimidazole fluorinated polyimide gel; then, the microspheres were first frozen in liquid nitrogen for 0.5 h, and then freeze-dried in a cold trap of a freeze dryer at a vacuum degree of 20 Pa at -50°C for 24 h, so that the benzimidazole fluorinated polyimide gel was converted into an aerogel and coated on the surface of the PPS@PDA microspheres, thereby obtaining interface-modified polyphenylene sulfide particles;

[0048] (S3) 75 parts of interface modified polyphenylene sulfide particles are mixed with 5 parts of polytetrafluoroethylene particles, 10 parts of glass fibers, and 0.2 parts of lubricant methyl silicone oil, and then mixed and extruded through a twin-screw extruder (a total of 6 working zones, zone 1: 280°C, zone 2: 300°C, zone 3: 310°C, zone 4: 320°C, zone 5: 300°C, zone 6: 290°C) and granulated to obtain a wear-resistant and self-lubricating polyphenylene sulfide-based composite material.

[0049] Example 2

[0050] The rest is the same as Example 1, except that: the amount of dopamine used in step (S1) is 2 g, and the amount of benzimidazole fluorinated polyimide gel a prepared in Preparation Example 1 in step (S2) is 25 parts.

[0051] Example 3

[0052] The rest is the same as Example 1, except that: the amount of dopamine used in step (S1) is 3 g, and the amount of benzimidazole fluorinated polyimide gel a prepared in Preparation Example 1 in step (S2) is 30 parts.

[0053] Example 4

[0054] The rest is the same as Example 1, except that: in step (S2), the benzimidazole-based fluorinated polyimide gel b prepared in Preparation Example 2 is used to replace the benzimidazole-based fluorinated polyimide gel a prepared in Preparation Example 1.

[0055] Example 5

[0056] The rest is the same as Example 1, except that in step (S3), the amount of each material used is: 90 parts of interface modified polyphenylene sulfide particles, 10 parts of polytetrafluoroethylene particles, 20 parts of glass fibers, and 1 part of lubricant methyl silicone oil.

[0057] Comparative Example 1

[0058] The rest is the same as Example 1, except that: step (S1) is omitted, and polyphenylene sulfide particles are used instead of PPS@PDA microspheres in step (S2), that is, polyphenylene sulfide is not polymerized on its surface by dopamine.

[0059] Comparative Example 2

[0060] The rest is the same as Example 1, except that in step (S2), the polyimide gel prepared in Comparative Preparation Example 1 is used to replace the benzimidazole-based fluorinated polyimide gel a prepared in Preparation Example 1.

[0061] Testing and analysis

[0062] The polyphenylene sulfide-based composite materials obtained in the above examples and comparative examples were subjected to the following performance tests:

[0063] Tensile strength: tested in accordance with national standard GB / T1040;

[0064] Impact strength: tested in accordance with national standard GB / T1843;

[0065] Friction coefficient and wear rate: tested using M-200 ring-block test bench in accordance with national standard GB / T3960-2016. Test conditions: room temperature, friction pair is titanium alloy ring, initial end surface roughness Ra = 0.25μm, test load 100N load, sliding speed 0.5m / s, friction and wear test time 3h.

[0066] The test results are shown in Table 1.

[0067] Table 1 Performance test of polyphenylene sulfide based composite materials

[0068]

[0069]

[0070] It can be seen from Table 1 that the polyphenylene sulfide-based composite material prepared by the present invention has excellent wear resistance and mechanical strength while maintaining a low friction coefficient.

Claims

1. A self-lubricating and wear-resistant polyphenylene sulfide-based composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 75-90 parts of interface-modified polyphenylene sulfide particles, 5-10 parts of polytetrafluoroethylene particles, 10-20 parts of reinforcing fibers, and 0.2-1 parts of lubricants; the interface-modified polyphenylene sulfide particles are prepared by polymerizing dopamine on the surface of polyphenylene sulfide particles to form polyphenylene sulfide@polydopamine (PPS@PDA) microspheres, coating the microspheres with benzimidazole fluorinated polyimide gel, and then freeze-drying the microspheres to form a composite phase interface; the amount of dopamine used is 1-3wt% of the polyphenylene sulfide particles; the amount of benzimidazole fluorinated polyimide gel used is 20-30wt% of the PPS@PDA microspheres.

2. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The dosage of dopamine is 2-3 wt% of the polyphenylene sulfide particles; the dosage of benzimidazole fluorinated polyimide gel is 25-30 wt% of the PPS@PDA microspheres.

3. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The benzimidazole fluorinated polyimide gel is obtained by reacting fluorinated dianhydride, benzimidazole diamine and 1,3,5-benzenetricarboxylic acid chloride to obtain benzimidazole fluorinated polyamic acid, and then imidizing the obtained benzimidazole fluorinated polyamic acid; the molar ratio of the fluorinated dianhydride, benzimidazole diamine and 1,3,5-benzenetricarboxylic acid chloride is 1:(1.05-1.15):(0.01-0.02); the reaction is carried out in a polar organic solvent, and the polar organic solvent accounts for 55-70wt%.

4. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 3, characterized in that: The fluorinated dianhydride is selected from at least one of 4,4'-hexafluoroisopropylidenephthalic anhydride (6FDA) and 4,4'-[2,2,2-trifluoro-1-(3-trifluoromethyl-phenyl)ethylene]diphthalic anhydride (TFDA); the benzimidazole diamine is selected from at least one of benzimidazole-1,2-diamine, 1H-benzo[D]imidazole-5,6-diamine, 1H-benzo[D]imidazole-2,5-diamine, 1H-benzo[D]imidazole-2,7-diamine, and 5,6-dimethyl-1H-benzo[D]imidazole-4,7-diamine; and the polar organic solvent is at least one of N,N'-dimethylacetamide (DMAC), N,N'-dimethylformamide (DMF), and N-methylpyrrolidone (NMP).

5. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The benzimidazole fluorinated polyimide gel is prepared by a preparation method comprising the following steps: (P1) Under an inert atmosphere, a benzimidazole diamine is dissolved in a polar organic solvent, and a fluorinated dianhydride is added to carry out a pre-condensation reaction at 5 to 10° C. for 4 to 6 hours, and then 1,3,5-benzenetricarboxylic acid chloride is added to continue the reaction for 0.5 to 1 hour to obtain a benzimidazole fluorinated polyamic acid solution; (P2) adding a water-carrying agent to a benzimidazole fluorinated polyamic acid solution, heating to 180-220° C. to carry out an imide condensation reaction until no water is discharged, cooling to room temperature and aging to obtain a benzimidazole fluorinated polyimide gel.

6. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The number average molecular weight of the polyphenylene sulfide is 30,000 to 50,000.

7. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The interface-modified polyphenylene sulfide particles are prepared by a preparation method comprising the following steps: (S1) adding polyphenylene sulfide particles and dopamine into a Tris-HCl buffer solution, stirring and reacting at 20-30° C. for 4-8 hours, and after the reaction is completed, centrifuging, washing, and drying to obtain polydopamine-modified polyphenylene sulfide particles, namely, PPS@PDA microspheres; (S2) PPS@PDA microspheres and benzimidazole fluorinated polyimide gel are stirred and mixed in a rolling ball machine so that the surface of the PPS@PDA microspheres is coated with a layer of benzimidazole fluorinated polyimide gel; and then the microspheres are freeze-dried so that the benzimidazole fluorinated polyimide gel is converted into aerogel and coated on the surface of the PPS@PDA microspheres, thereby obtaining interface-modified polyphenylene sulfide particles.

8. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 7, characterized in that: In step (S1), the concentration of the Tris-HCl buffer solution is 10-30 mM, and the pH is 8.0-9.0; the volume ratio of the mass of the dopamine to the Tris-HCl buffer solution is 1-3 g:1000 mL; the drying is performed in a vacuum oven at 60-80° C. for 12-24 h; and / or In step (S2), the stirring and mixing conditions are: the ball rolling machine speed is 100-200 rpm, and the time is 1-2 hours; the freeze-drying conditions are: first freezing in liquid nitrogen for 0.5-1 hour, and then vacuum drying in a cold trap at -50--40°C for 24-48 hours, and the vacuum degree is 10-30 Pa.

9. The self-lubricating and wear-resistant polyphenylene sulfide-based composite material according to claim 1, characterized in that: The particle size of the interface modified polyphenylene sulfide particles is 10 to 60 μm, and the particle size of the polytetrafluoroethylene particles is 5 to 15 μm; and / or The reinforcing fiber is at least one of glass fiber, carbon fiber, chopped aramid fiber, and basalt fiber; the reinforcing fiber has a diameter of 2 to 10 μm and a length of 1 to 3 mm; and / or The lubricant is at least one of amino silicone oil, methyl silicone oil, ethyl silicone oil and polyether modified silicone oil.

10. The method for preparing the wear-resistant self-lubricating polyphenylene sulfide-based composite material according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing interface-modified polyphenylene sulfide particles with polytetrafluoroethylene particles, reinforcing fibers and lubricants, and then mixing and extruding to obtain a wear-resistant self-lubricating polyphenylene sulfide-based composite material; Preferably, the mixing and extruding is carried out in a twin-screw extruder at an extrusion temperature of 280-320° C.; and granulation is further included after the mixing and extruding.

Citation Information

Patent Citations

  • Polyphenylene sulfide-based self-lubricating multi-component composite material and preparation method thereof

    CN114085529A

  • Aerogel / polyphenylene sulfide self-lubricating friction material and preparation method thereof

    CN115785671A

  • Polyphenylene sulfide material with low friction coefficient and preparation method thereof

    CN116925547A

  • Wear-resistant polyphenylene sulfide material and preparation method thereof

    CN117050523A

  • High-temperature-resistant low-friction polyphenylene sulfide particles and preparation method thereof

    CN117210006A