Material for tent pole and preparation method thereof
By using a combination of materials such as glass fiber and phosphophenyl biphenylsulfone-based polymers, the weather resistance and impact toughness of tent poles are improved, and the problem of insufficient performance of existing tent poles is solved, achieving simple process and low cost production effect.
Patent Information
- Application Number
- CN202411256089.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
AI Technical Summary
The weather resistance and impact toughness of existing tent poles materials are insufficient, the mechanical and mechanical properties need to be improved, and the preparation process is complex and the cost is high.
The materials for tents composed of glass fiber, phosphophenyl biphenylsulfone polymer, methylphenyl vinyl silicone rubber, etc. are prepared through injection molding process, and the types and dosage of raw materials are reasonably proportioned to make the materials. Improve weather resistance and mechanical mechanical properties under electron effects, steric hindrance effects and conjugation effects.
The weather resistance and impact toughness of the tent pole materials have been significantly improved, the process is simple and convenient to operate, and it is suitable for continuous large-scale production, reducing the preparation cost.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a material for tent poles and a preparation method thereof. Background Art
[0002] Tents are essential for outdoor activities, mountaineering, and disaster relief. They are compact and easy to carry when folded, and can provide people with a warm and comfortable resting space, sheltering from wind and rain. The tent pole is the frame of the tent, and the quality of the frame material affects not only the life of the tent, but also the stability of the tent. Therefore, it is particularly important to develop tent pole materials with excellent comprehensive performance and performance stability.
[0003] At present, the common materials for outdoor tent poles include metal materials and glass fiber reinforced composite materials. Metal materials have more or less defects such as heavy weight, easy corrosion, limited toughness and fatigue resistance. Glass fiber reinforced composite materials have become one of the mainstream products of tent pole materials due to their advantages such as high specific strength, good corrosion resistance and durability. However, glass fiber reinforced composite materials on the market still have more or less technical defects such as insufficient weather resistance, mechanical properties and impact toughness need to be further improved.
[0004] In order to solve the above technical problems, a Chinese invention patent with authorization announcement number CN105113846B discloses a highly wear-resistant tent support pole and a production process, wherein the support pole for an outdoor tent comprises a metal support pole and a support pole coating arranged on the outside of the metal support pole, wherein the support pole coating is provided with powder material, metal coating, wear-resistant coating, transition layer and metal coating in sequence from the inside to the outside, and the mass fractions of each component in the metal support pole include 4-5 parts of C, 1-2.5 parts of Cu, 5-8 parts of Mn, 1-3 parts of Ti, 63-67 parts of Fe, 1-2.5 parts of Cr, 2-3 parts of Al, 2-4 parts of Co, 1.7-3.7 parts of Si, 1.5-2.5 parts of Sn, and 1-3 parts of Ni; the invention is a highly wear-resistant tent support pole and a production process with simple process, easy use and low production cost, which can effectively increase the toughness, heat resistance, corrosion resistance and wear resistance of the metal support pole, and the coating is more effectively adsorbed on the support pole, which can more effectively increase the adhesion of the coating. However, the material has a multi-layer structure, is prone to delamination, has a short service life, and has a high preparation cost.
[0005] It can be seen that the development of a tent pole material with sufficient weather resistance, excellent mechanical properties and impact toughness and a preparation method thereof meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the field of tent pole materials. Summary of the invention
[0006] In view of the above problems, the object of the present invention is to provide a material for tent poles having sufficient weather resistance, excellent mechanical properties and impact toughness, and a preparation method thereof.
[0007] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a material for tent poles is made of the following raw materials in parts by weight: 20-30 parts of glass fiber, 3-5 parts of coupling agent, 80-90 parts of phosphaphenanthryl biphenyl sulfone polymer, 0.8-1.5 parts of catalyst, 0.4-0.6 parts of antioxidant, 0.8-1.2 parts of lubricant, 3-5 parts of environmentally friendly plasticizer, 5-8 parts of methyl phenyl vinyl silicone rubber, 4,4'-diacyl chloride diphenyl ether 3-5 parts, 2,5-furandicarbonyl chloride 0.5-1 parts, 2,4,6-trivinyl cycloboroxine 3-5 parts, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide 1-3 parts, initiator 0.3-0.6 parts; the phosphaphenanthrene-based biphenyl sulfone-based polymer includes structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone).
[0008] Preferably, the glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, a brand of ER13-2000-988A, and is produced by China Jushi Group.
[0009] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0010] Preferably, the preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene are mixed evenly, and then added to a reactor connected to a water separator, and the air in the reactor is replaced with nitrogen. Under nitrogen protection, the reaction is stirred at 135-145° C. for 3-5 hours, and the water and toluene generated during the reaction are removed through the water separator. The temperature is then raised to 165-175° C., and the reaction is continued with stirring for 15-18 hours. Then, the temperature is cooled to room temperature, and the precipitated polymer is precipitated in water. The precipitated polymer is washed with ethanol for 3-6 times, and finally placed in a vacuum drying oven at 90-95° C. to dry to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer.
[0011] Preferably, the molar ratio of 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, di-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene is 1:1:(1-2):(10-20):4.
[0012] Preferably, the catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:(2-4).
[0013] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0014] Preferably, the lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide.
[0015] Preferably, the environmentally friendly plasticizer is epoxidized soybean oil.
[0016] Preferably, the methylphenylvinyl silicone rubber is 120 type methylphenylvinyl silicone rubber.
[0017] Preferably, the initiator is a mixture of dicumyl peroxide, benzoyl peroxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:(0.8-1.2):(1-2).
[0018] Another object of the present invention is to provide a method for preparing the tent pole material, comprising the following steps: mixing the raw materials evenly to obtain a mixed material, adding the mixed material to an injection molding machine, and performing injection molding to obtain the tent pole material.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The preparation method of the tent pole material disclosed in the present invention only requires the raw materials to be mixed evenly and then injection molded. The process is simple, the operation and control are convenient, the dependence on equipment and labor intensity are low, the impact on the environment is small, and it is suitable for continuous large-scale production and has a high value for promotion and application.
[0021] (2) The tent pole material disclosed in the present invention is made of the following raw materials in parts by weight: 20-30 parts of glass fiber, 3-5 parts of coupling agent, 80-90 parts of phosphaphenanthryl biphenyl sulfone polymer, 0.8-1.5 parts of catalyst, 0.4-0.6 parts of antioxidant, 0.8-1.2 parts of lubricant, 3-5 parts of environmentally friendly plasticizer, 5-8 parts of methyl phenyl vinyl silicone rubber, 3-5 parts of 4,4'-diacyl chloride diphenyl ether, 2, 0.5-1 part of 5-furandicarboxylic acid chloride, 3-5 parts of 2,4,6-trivinyl cycloboroxine, 1-3 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, and 0.3-0.6 parts of initiator; the phosphaphenanthrene-based biphenyl sulfone-based polymer includes structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone). Through the mutual cooperation between the raw materials, the material for the tent poles has sufficient weather resistance, excellent mechanical properties and impact toughness; through the reasonable selection of the types and dosage ratios of the above raw materials, phosphaphenanthrene groups, biphenyl sulfone groups, methylphenyl silicone rubber, phenyl ether, furan, cycloboroxane, cyano groups, fluorinated phenyl groups and amide groups are simultaneously introduced into the molecular structure of the material. Under the multiple effects of these groups such as electronic effect, steric effect and conjugation effect, the weather resistance of the manufactured material is more sufficient, and the mechanical properties and impact toughness are more excellent.
[0022] (3) The tent pole material disclosed in the present invention comprises a phosphaphenanthryl biphenyl sulfone-based polymer comprising the following monomer introduced structural units: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, bi-(4-chlorodiphenyl sulfone), and the phosphaphenanthryl, biphenyl sulfone and phenyl ether structures are simultaneously introduced into the polymer molecular structure, and the interaction between them can effectively improve the mechanical properties and weather resistance; by introducing methylphenyl vinyl silicone rubber, the toughness can be further improved; the raw material components containing unsaturated olefinic bonds can be copolymerized, and the acyl chloride groups on 4,4'-diacyl chloride diphenyl ether and 2,5-furandicarboxylic acid chloride can react with the benzene rings on the phosphaphenanthryl biphenyl sulfone-based polymer and the methylphenyl vinyl silicone rubber to form an interpenetrating network structure, thereby further improving the weather resistance, mechanical properties and impact toughness of the material. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.
[0024] Example 1
[0025] A material for tent poles is made of the following raw materials in parts by weight: 20 parts of glass fiber, 3 parts of coupling agent, 80 parts of phosphaphenanthryl biphenyl sulfone-based polymer, 0.8 parts of catalyst, 0.4 parts of antioxidant, 0.8 parts of lubricant, 3 parts of environmentally friendly plasticizer, 5 parts of methylphenyl vinyl silicone rubber, 3 parts of 4,4'-diacyl chloride diphenyl ether, 0.5 parts of 2,5-furan dicarboxylic acid chloride, 3 parts of 2,4,6-trivinyl cycloboroxane, 1 part of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.3 parts of initiator; the phosphaphenanthryl biphenyl sulfone-based polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, bi-(4-chlorodiphenyl sulfone).
[0026] The glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, with a brand name of ER13-2000-988A, and is produced by China Jushi Group; the coupling agent is a silane coupling agent KH550.
[0027] The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene are uniformly mixed, and then added into a reaction kettle connected with a water separator, and the air in the kettle is replaced with nitrogen. Under the protection of nitrogen, the reaction is stirred at 135°C for 3 hours, and the water and toluene generated in the reaction process are removed through the water separator, and then heated to 400 °C. The mixture was heated to 165°C, stirred and reacted for 15 hours, then cooled to room temperature, precipitated in water, and the precipitated polymer was washed with ethanol three times, and finally dried in a vacuum oven at 90°C to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide, and toluene was 1:1:1:10:4. The M of the polymer was measured by GPC test. n =14881 g / mol, M W / M n =1.357; calculated by elemental analysis and weight change, the molar ratio of the structural units introduced by 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide and di-(4-chlorodiphenyl sulfone) in the polymer is 1:1.
[0028] The catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:2; the antioxidant is antioxidant 1010; the lubricant is pentaerythritol stearate; the environmentally friendly plasticizer is epoxidized soybean oil; the methylphenyl vinyl silicone rubber is 120 type methylphenyl vinyl silicone rubber, provided by Anhui Aiyota Silicone Oil Co., Ltd.; the initiator is a mixture of diisopropyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:0.8:1.
[0029] A method for preparing the tent pole material comprises the following steps: mixing various raw materials evenly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the tent pole material.
[0030] Example 2
[0031] A material for tent poles is made of the following raw materials in parts by weight: 23 parts of glass fiber, 3.5 parts of coupling agent, 82 parts of phosphaphenanthryl biphenyl sulfone-based polymer, 1 part of catalyst, 0.45 parts of antioxidant, 0.9 parts of lubricant, 3.5 parts of environmentally friendly plasticizer, 6 parts of methylphenyl vinyl silicone rubber, 3.5 parts of 4,4'-diacyl chloride diphenyl ether, 0.6 parts of 2,5-furan dicarboxylic acid chloride, 3.5 parts of 2,4,6-trivinyl cycloboroxane, 1.5 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.4 parts of initiator; the phosphaphenanthryl biphenyl sulfone-based polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, bi-(4-chlorodiphenyl sulfone).
[0032] The glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, with a brand name of ER13-2000-988A, and is produced by China Jushi Group; the coupling agent is a silane coupling agent KH560.
[0033] The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: uniformly mixing 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene, adding the mixture to a reaction kettle connected to a water separator, replacing the air in the kettle with nitrogen, stirring and reacting at 137° C. for 3.5 hours under nitrogen protection, removing water and toluene generated during the reaction process through the water separator, then heating to 168° C., and continuing to stir and react for 16 hours. Then cool to room temperature, precipitate in water, wash the precipitated polymer with ethanol for 4 times, and finally dry in a vacuum drying oven at 92° C. to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide, and toluene is 1:1:1.2:12:4; the catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:2.5.
[0034] The antioxidant is antioxidant 1076; the lubricant is ethylene bisstearamide; the environmentally friendly plasticizer is epoxidized soybean oil; the methylphenyl vinyl silicone rubber is 120 type methylphenyl vinyl silicone rubber, provided by Anhui Aiyota Silicone Oil Co., Ltd.; the initiator is a mixture of diisopropyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:0.9:1.2.
[0035] A method for preparing the tent pole material comprises the following steps: mixing various raw materials evenly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the tent pole material.
[0036] Example 3
[0037] A material for tent poles is made of the following raw materials in parts by weight: 25 parts of glass fiber, 4 parts of coupling agent, 85 parts of phosphaphenanthryl biphenyl sulfone-based polymer, 1.2 parts of catalyst, 0.5 parts of antioxidant, 1 part of lubricant, 4 parts of environmentally friendly plasticizer, 6.5 parts of methylphenyl vinyl silicone rubber, 4 parts of 4,4'-diacyl chloride diphenyl ether, 0.8 parts of 2,5-furan dicarboxylic acid chloride, 4 parts of 2,4,6-trivinyl cycloboroxane, 2 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.45 parts of initiator; the phosphaphenanthryl biphenyl sulfone-based polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide and bi-(4-chlorodiphenyl sulfone).
[0038] The glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, with a brand name of ER13-2000-988A, and is produced by China Jushi Group; the coupling agent is a silane coupling agent KH570.
[0039] The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene are uniformly mixed, and then added into a reaction kettle connected with a water separator, and the air in the kettle is replaced with nitrogen. Under the protection of nitrogen, the reaction is stirred at 140°C for 4 hours, and the water and toluene generated in the reaction process are removed through the water separator, and then the temperature is raised to 170 ° C, continue to stir the reaction for 16.5 hours, then cool to room temperature, precipitate in water, wash the precipitated polymer with ethanol 5 times, and finally place it in a vacuum drying oven at 93 ° C to dry to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, di-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide, and toluene is 1:1:1.5:15:4.
[0040] The catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:3; the antioxidant is antioxidant 168; the lubricant is pentaerythritol stearate; the environmentally friendly plasticizer is epoxidized soybean oil; the methylphenyl vinyl silicone rubber is 120 type methylphenyl vinyl silicone rubber, provided by Anhui Aiyota Silicone Oil Co., Ltd.; the initiator is a mixture of diisopropyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1:1.5.
[0041] A method for preparing the tent pole material comprises the following steps: mixing various raw materials evenly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the tent pole material.
[0042] Example 4
[0043] A material for tent poles is made of the following raw materials in parts by weight: 28 parts of glass fiber, 4.5 parts of coupling agent, 88 parts of phosphaphenanthryl biphenyl sulfone polymer, 1.4 parts of catalyst, 0.55 parts of antioxidant, 1.1 parts of lubricant, 4.5 parts of environmentally friendly plasticizer, 7.5 parts of methylphenyl vinyl silicone rubber, 4.5 parts of 4,4'-diacyl chloride diphenyl ether, 0.9 parts of 2,5-furan dicarboxylic acid chloride, 4.5 parts of 2,4,6-trivinyl cycloboroxane, 2.5 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.55 parts of initiator; the phosphaphenanthryl biphenyl sulfone polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide and bi-(4-chlorodiphenyl sulfone).
[0044] The glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, and is produced by China Jushi Group with a brand name of ER13-2000-988A; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:2:3.
[0045] The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene are uniformly mixed, and then added into a reaction kettle connected with a water separator, and the air in the kettle is replaced with nitrogen. Under the protection of nitrogen, the reaction is stirred at 143°C for 4.5 hours, and the water and toluene generated in the reaction process are removed through the water separator, and then the temperature is raised. to 173° C., continue stirring to react for 17.5 hours, then cool to room temperature, precipitate in water, wash the precipitated polymer with ethanol 5 times, and finally dry in a vacuum drying oven at 94° C. to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide, and toluene is 1:1:1.8:19:4.
[0046] The catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:3.5; the antioxidant is a mixture of antioxidant 1010, antioxidant 1076, and antioxidant 168 in a mass ratio of 1:1:2; the lubricant is a mixture of pentaerythritol stearate and ethylene bisstearamide in a mass ratio of 3:5; the environmentally friendly plasticizer is epoxy soybean oil; the methyl phenyl vinyl silicone rubber is 120 type methyl phenyl vinyl silicone rubber, provided by Anhui Aiyota Silicone Oil Co., Ltd.; the initiator is a mixture of diisopropyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1.1:1.8.
[0047] A method for preparing the tent pole material comprises the following steps: mixing various raw materials evenly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the tent pole material.
[0048] Example 5
[0049] A material for tent poles is made of the following raw materials in parts by weight: 30 parts of glass fiber, 5 parts of coupling agent, 90 parts of phosphaphenanthryl biphenyl sulfone-based polymer, 1.5 parts of catalyst, 0.6 parts of antioxidant, 1.2 parts of lubricant, 5 parts of environmentally friendly plasticizer, 8 parts of methylphenyl vinyl silicone rubber, 5 parts of 4,4'-diacyl chloride diphenyl ether, 1 part of 2,5-furan dicarboxylic acid chloride, 5 parts of 2,4,6-trivinyl cycloboroxane, 3 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.6 parts of initiator; the phosphaphenanthryl biphenyl sulfone-based polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide, bi-(4-chlorodiphenyl sulfone).
[0050] The glass fiber is an alkali-free continuous glass fiber with a single filament diameter of 13 μm and a length of 1-3 mm, with a brand name of ER13-2000-988A, and is produced by China Jushi Group; the coupling agent is a silane coupling agent KH550.
[0051] The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene are uniformly mixed, and then added into a reaction kettle connected with a water separator, and the air in the kettle is replaced with nitrogen. Under the protection of nitrogen, the reaction is stirred at 145°C for 5 hours, and the water and toluene generated in the reaction process are removed through the water separator, and then heated to 400 °C. The mixture was heated to 175° C., stirred and reacted for 18 hours, then cooled to room temperature, precipitated in water, washed with ethanol for 6 times, and finally dried in a vacuum drying oven at 95° C. to constant weight to obtain a phosphaphenanthrene-based biphenyl sulfone-based polymer; the molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide, and toluene was 1:1:2:20:4.
[0052] The catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:4; the antioxidant is antioxidant 1010; the lubricant is ethylene bisstearamide; the environmentally friendly plasticizer is epoxidized soybean oil; the methyl phenyl vinyl silicone rubber is 120 methyl phenyl vinyl silicone rubber, provided by Anhui Aiyota Silicone Oil Co., Ltd.; the initiator is a mixture of diisopropyl peroxide, benzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:1.2:2.
[0053] A method for preparing the tent pole material comprises the following steps: mixing various raw materials evenly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the tent pole material.
[0054] Comparative Example 1
[0055] A material for tent poles and a preparation method thereof, which is substantially the same as Example 1, except that 4,4'-diacyl chloride diphenyl ether and N-(4-cyano-3-trifluoromethylphenyl) methacrylamide are not added.
[0056] Comparative Example 2
[0057] A material for tent poles and a preparation method thereof, which is substantially the same as Example 1, except that 2,5-furandicarbonyl chloride and 2,4,6-trivinyl cycloboroxine are not added.
[0058] In order to further illustrate the unexpected positive technical effects achieved by the products of each embodiment of the present invention, the relevant performance tests were conducted on the materials for tent poles made in each example. The test results are shown in Table 1. During the test, the molding temperature of the injection molding machine was 285° C., the injection pressure was 100 MPa, and the test method was as follows:
[0059] (1) Tensile properties: The tensile properties were tested according to the method in ASTM D412.
[0060] (2) Notched impact strength: refer to GB / T1043-2008 standard, the method name is GB / T1043.1 / 1eA, the specimen type is 1, the impact direction is lateral, and the notch type is A.
[0061] (3) Weather resistance: The carbon arc lamp aging test was carried out according to GB / T16422.4-1996, using a continuous 720h lighting test, a blackboard temperature of (65±3)°C, and a relative humidity of (50±5)%. The tensile strength retention rate of the product was measured, tensile strength retention rate = tensile strength after aging / tensile strength before aging × 100%. The greater the tensile strength retention rate, the better the weather resistance.
[0062] Table 1
[0063] project Tensile Strength Notched impact strength Weather resistance unit MPa <![CDATA[KJ / m 2 ]]> % Example 1 83.5 26.3 99.07 Example 2 84.7 27.0 99.19 Example 3 86.2 27.5 99.38 Example 4 87.2 28.5 99.63 Example 5 88.0 29.2 99.93 Comparative Example 1 75.2 22.1 96.46 Comparative Example 2 71.1 20.7 97.09
[0064] It can be seen from Table 1 that the tent pole material disclosed in the embodiment of the present invention has better mechanical properties, weather resistance and impact toughness than the comparative example product; the addition of 4,4'-diacyl chloride diphenyl ether, N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, 2,5-furandicarboxylic acid chloride and 2,4,6-trivinyl cycloboroxine is beneficial to improving the above properties.
[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as described above. However, any technician familiar with the profession can make some changes, modifications and evolutions of the technical content disclosed above without departing from the scope of the technical solution of the present invention, which are all equivalent embodiments of the present invention. At the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A material for tent poles, characterized in that: The invention is prepared from the following raw materials in parts by weight: 20-30 parts of glass fiber, 3-5 parts of coupling agent, 80-90 parts of phosphaphenanthryl biphenyl sulfone-based polymer, 0.8-1.5 parts of catalyst, 0.4-0.6 parts of antioxidant, 0.8-1.2 parts of lubricant, 3-5 parts of environmentally friendly plasticizer, 5-8 parts of methylphenyl vinyl silicone rubber, 3-5 parts of 4,4'-diacyl chloride diphenyl ether, 0.5-1 parts of 2,5-furan dicarboxylic acid chloride, 3-5 parts of 2,4,6-trivinyl cycloboroxane, 1-3 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, and 0.3-0.6 parts of initiator; the phosphaphenanthryl biphenyl sulfone-based polymer comprises structural units introduced by the following monomers: 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthryl-10-oxide and bi-(4-chlorodiphenyl sulfone).
2. The material for tent poles according to claim 1, characterized in that: The glass fiber is an alkali-free continuous glass fiber with a single fiber diameter of 13 μm, a length of 1-3 mm, and a brand of ER13-2000-988A.
3. The material for tent poles according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
4. The material for tent poles according to claim 1, characterized in that: The preparation method of the phosphaphenanthrene-based biphenyl sulfone-based polymer comprises the following steps: uniformly mixing 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, bi-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene, adding the mixture to a reaction kettle connected to a water separator, replacing the air in the kettle with nitrogen, stirring and reacting at 135-145° C. for 3-5 hours under nitrogen protection, removing water and toluene generated during the reaction process through the water separator, then heating to 165-175° C., continuing to stir and react for 15-18 hours, cooling to room temperature, precipitating the mixture in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying the mixture in a vacuum drying oven at 90-95° C. to constant weight to obtain the phosphaphenanthrene-based biphenyl sulfone-based polymer.
5. The material for tent poles according to claim 4, characterized in that: The molar ratio of the 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, di-(4-chlorodiphenyl sulfone), cesium carbonate, dimethyl sulfoxide and toluene is 1:1:(1-2):(10-20):
4.
6. The material for tent poles according to claim 1, characterized in that: The catalyst is a mixture of anhydrous zinc chloride and anhydrous ferric chloride in a mass ratio of 1:(2-4); the antioxidant is at least one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
7. The material for tent poles according to claim 1, characterized in that: The lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide; and the environmentally friendly plasticizer is epoxidized soybean oil.
8. The material for tent poles according to claim 1, characterized in that: The methyl phenyl vinyl silicone rubber is 120 type methyl phenyl vinyl silicone rubber.
9. The material for tent poles according to claim 1, wherein: The initiator is a mixture of dicumyl peroxide, benzoyl peroxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane in a mass ratio of 1:(0.8-1.2):(1-2).
10. A method for preparing the material for tent poles according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing various raw materials uniformly to obtain a mixed material, adding the mixed material into an injection molding machine, and performing injection molding to obtain the material for tent poles.
Citation Information
Patent Citations
Hyperbranched poly(aryl ether ketone), preparation method and application thereof in viscosity modifier
CN101357985A
Carbon fiber based composite material fishing rod and preparation method thereof
CN109306178A
Sizing agent for improving tensile strength and toughness of glass fibers and preparation method thereof
CN112479604A
High-strength and high-toughness tent support rod material and preparation method thereof
CN115181385A
Preparation method of 9, 10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide
CN118373852A