Modified asphalt and preparation method of ultra-thin and ultra-thin layer asphalt for low-temperature construction

Through low-temperature construction technology and modified asphalt formula, the problem of insufficient high-temperature construction and crack resistance in the existing technology is solved, and the extremely thin and ultra-thin layer of asphalt with high flow, crack resistance and environmental protection is achieved, which is suitable for a wider range of Application scenarios and reduce workers' health and environmental risks.

CN119060549APending Publication Date: 2024-12-03SICHUAN JINGLU ROAD MATERIALS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310600889.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing hot-mixed high-viscosity and high elastic asphalt ultra-thin layer technology has high equipment and construction ambient temperature requirements, poor crack resistance after asphalt aging, thickness limits the application seasonality and scenarios, and untimely crushing and easy to cause blockages. question.

Method used

Using low-temperature construction technology, the formulation and preparation methods of first-order and second-order modified asphalt are added, and the components such as rock asphalt, SBS, SBR, and tung oil are respectively added, and the liquid nitrogen is deeply cold crushed to produce high fluidity and high Extremely thin ultra-thin layer of asphalt with softening points, high ductility and high toughness, suitable for low-temperature construction.

Benefits of technology

It realizes low-temperature construction, reduces the temperature requirements of equipment and construction ambient, improves the crack resistance of asphalt, extends service life, reduces material use and emissions, is suitable for a wider range of application scenarios, and reduces workers' health risks and greenhouses Gas emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to ultra-thin ultra-thin layer asphalt as well as a preparation method and a construction process thereof. The ultra-thin ultra-thin layer asphalt is prepared from 92 to 95 parts of second-order modified asphalt, 20 parts of polyoxyethylene ether, 30 parts of polyoxypropylene ether, 3 parts of toluene diisocynate, 10 parts of hexamethylene diisocyanate, 0.02 part of dibutyltin dilaurate, 20 parts of butyl epoxy modified silicone oil, 16.98 parts of distilled water and the like. And heating, mixing and shearing. The modified asphalt provided by the invention has the advantages of high fluidity, high softening point, high ductility and high toughness. The method is suitable for the ultrathin wearing layer with the structural layer thickness of 1-1.5 cm, has small influence on the vertical elevation, and saves raw materials. And the ultrathin layer can be paved when the construction temperature is higher than-5 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road maintenance, in particular to a modified asphalt, in particular to an ultra-thin layer of asphalt constructed at low temperature and a preparation method thereof. Background Art

[0002] With the development of economic construction, my country's road construction industry has also begun to shift from the incremental market of "large-scale construction" to the stock market that focuses on maintenance and pre-maintenance. From the perspective of maintenance strategy, pavement pre-maintenance is to conduct regular road condition surveys, use relevant detection technologies to analyze road conditions before the road has any diseases, find out the hidden diseases of the road in advance, and adopt a systematic cost-effective maintenance strategy to prevent the expansion of invisible diseases, slow down the deterioration of pavement performance, and delay the arrival of major and medium repair cycles, thereby extending the overall service life of the pavement and maintaining the road network in an acceptable service state. At present, the main pre-maintenance methods are: fog seal, micro-surfacing, and thin layer overlay. The pre-maintenance technology of thin layer overlay with a thickness of less than 2.5cm has been widely used at home and abroad. In the 1970s, France pioneered the thin-layer overlay technology, and successively launched 3-5 cm thick asphalt concrete surface layer (BBM), 2-3 cm thick thin layer asphalt concrete (BBTM), and ultra-thin wear layer (Novachip) with a minimum paving thickness of 20 mm. In the 1990s, the United States developed an open-graded anti-skid wear layer (OGFC) to replace the traditional road surface treatment technology. Due to the regional incompatibility and high patent cost of foreign technology in the promotion process in my country, China has been competing to break the monopoly and develop and apply ultra-thin wear layers, such as SMA-8 high-toughness ultra-thin wear, UAT-10 super wear layer, etc. From the perspective of road public asset preservation and resident travel service level, the adoption of thin-layer overlay pre-maintenance is the most reasonable choice for highway management departments and construction departments, but there are still some problems that need to be solved, such as the lack of unified specification requirements, controversial key performance indicators, lack of industry consensus, etc. Therefore, the present invention proposes a low-carbon, green, environmentally friendly and economical low-temperature construction technology for ultra-thin asphalt technology for preventive maintenance of pavement.

[0003] The defects of the current hot mix high viscosity and high elastic asphalt ultra-thin layer are:

[0004] (1) The discharge temperature is 180 degrees Celsius and the initial pressure temperature is 150 degrees Celsius, which places extremely high requirements on the equipment and construction environment temperature.

[0005] (2) The indicators of asphalt after aging cannot meet the requirements of low-temperature crack resistance and other properties.

[0006] (3) The thickness of the ultra-thin layer of hot-mixed high-viscosity and high-elastic asphalt is generally 1.5-2.5cm.

[0007] (4) After the rolling temperature requirements are high, if the rolling is not timely, it is easy to cause large areas of thin layers to fall off.

[0008] (5) It limits the application seasonality and application scenarios of ultra-thin products. Summary of the invention

[0009] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide an ultra-thin layer of asphalt for low-temperature construction and a preparation method. For preventive maintenance of pavement, a low-carbon, green, environmentally friendly and economical ultra-thin layer of low-temperature construction technology is proposed.

[0010] The first object of the present invention is to provide a first-stage modified asphalt, which is composed of the following quality components:

[0011] 85-90 parts of base asphalt

[0012] 10-15 parts of first-stage modifier

[0013] The first-order modifier is composed of the following mass components:

[0014] 5-8 parts rock asphalt

[0015] SBS 65 parts

[0016] SBR 20-25 parts

[0017] 5-7 parts tung oil

[0018] The base asphalt is heated to between 160-180°C, preferably 170-180°C, and the first-order modifier is added and mixed, the mixture is pressed and sheared, and the mixture is cryogenically ground into powder by liquid nitrogen to obtain the first-order modified asphalt. The powder particle size is preferably less than or equal to 200 mesh.

[0019] The second object of the present invention is to provide a second-stage modified asphalt, which is composed of the following quality components:

[0020] First-stage modified asphalt 86.5-91.5 parts

[0021] Sulfur: 0.5 parts

[0022] Silicone oligomer: 3-8 parts

[0023] Second stage modifier: 5 parts

[0024] The second-stage modifier is composed of the following mass components:

[0025] 25-30 parts of tung oil

[0026] Epoxidized soybean oil 8-12 parts

[0027] Phthalic anhydride 20-30 parts

[0028] Pentaerythritol 12-20 parts

[0029] 3-6 parts of glycerol

[0030] 3-5 parts of C9 petroleum resin

[0031] C5 petroleum resin 5-7 parts

[0032] C10 petroleum resin 6-8 parts

[0033] 2-4 parts of acrylic acid

[0034] 2-4 parts of resin catalyst;

[0035] The first-stage asphalt is heated to between 160-190°C, preferably 170-180°C, and then sulfur, silicone oligomer and second-stage modifier are added, and the mixture is pressed and sheared to obtain the product.

[0036] The third object of the present invention is to provide an ultra-thin layer of asphalt, wherein the asphalt is composed of the following mass components:

[0037] Second stage modified asphalt 92-95

[0038] Active agent 5-8 parts

[0039] The active agent is composed of the following mass components:

[0040] 20 parts of polyoxyethylene ether

[0041] 30 parts of polyoxypropylene ether

[0042] 3 parts of toluene diisocyanate

[0043] Hexamethylene diisocyanate 10 parts

[0044] 0.02 parts of dibutyltin dilaurate

[0045] 20 parts of butyl epoxy modified silicone oil

[0046] 16.98 parts of distilled water

[0047] The second-stage asphalt is heated to between 140-160°C, an activator is added, and the mixture is pressed and sheared to obtain the product.

[0048] The fourth object of the present invention is to provide a method for preparing an ultra-thin layer of asphalt:

[0049] S1 prepares the first-order modifier, second-order modifier and active agent according to the ratio.

[0050] S2 heats the base asphalt to 160-180℃

[0051] S3 adding the first-order modifier to the base asphalt obtained in step 2 and mixing thoroughly;

[0052] S4 cuts the mixture into tablets,

[0053] S5 obtains the first-order modified asphalt by deep-cryogenic crushing of the sheared fragments;

[0054] S6 heats the first-stage modified asphalt to 160-180°C;

[0055] S7: adding sulfur, organosilicon oligomer and second-stage modifier to the first-stage modified asphalt obtained in step 6 and mixing for 0.5-1h;

[0056] S8 compresses and shears the mixture to obtain a second-stage modified asphalt;

[0057] S9 heats the second-stage modified asphalt to 140-160°C;

[0058] S10: adding the active agent to the second-stage modified asphalt obtained in step 9 and mixing for 0.5-1h;

[0059] S11 is to press the mixture into tablets by shearing.

[0060] As a further improvement, the cooling temperature in the above-mentioned deep cold crushing treatment step is -130°C-150°C.

[0061] The preparation method of the above-mentioned second-stage modifier is as follows:

[0062] The raw materials are reacted in a reactor at 120-160° C. for 6-10 hours to obtain the product.

[0063] The preparation method of the above active agent is as follows:

[0064] S1 Add polyoxyethylene ether and polyoxypropylene ether into the reaction kettle and stir, raise the temperature to 50℃-80℃,

[0065] S2 then adds dibutyltin dilaurate, epoxy modified silicone oil, toluene diisocyanate, and hexamethylene diisocyanate, and mixes and stirs for 0.5h-1h.

[0066] Add distilled water to S3 and cool to room temperature.

[0067] The present invention also relates to a construction method for an ultra-thin layer of asphalt used for low-temperature construction: the thickness of the asphalt concrete to be constructed is 0.7-1.5 cm, and the construction temperature is above minus 5°C.

[0068] The first-stage modified asphalt obtained by the present invention is a composite modified high-viscosity and high-elastic asphalt, and compared with the prior art, the needle penetration is reduced by about 16, and the softening point is increased by 20° C. The second-stage modified asphalt obtained by the present invention is a composite high-ductility, high-viscosity and high-elastic asphalt, and the viscosity is reduced compared with the first-stage modified asphalt.

[0069] Compared with the prior art, the ultra-thin layer of asphalt obtained by the present invention has the following beneficial effects:

[0070] (1) The ultra-thin asphalt for low-temperature construction of the present invention is based on a special multi-modified asphalt, which is a modified asphalt with high fluidity, high softening point, high ductility and high toughness.

[0071] (2) The discharge temperature of the mixed material is 130-140°C.

[0072] (3) There is no need to roughen or mill the original cement pavement or asphalt pavement layer.

[0073] (4) No synchronous paver is required, asynchronous paver can be used for construction.

[0074] (5) The initial pressure can be 70℃ and the final pressure can be above 50℃.

[0075] (6) Use non-emulsified non-stick wheel with special waterproof adhesive layer.

[0076] (7) The ultra-thin wear layer with a suitable structural layer thickness of 1 to 1.5 cm has little impact on the vertical elevation and saves raw materials.

[0077] (8) The ultra-thin layer can be laid at a construction temperature above -5°C.

[0078] (9) Traffic can be opened quickly and traffic control time is short. The paving can be opened after the paving temperature drops to 40℃.

[0079] (10) It greatly reduces the emission of asphalt fumes, protects the health of workers, is more environmentally friendly, and is more in line with the national green environmental protection policy. It can save 20-30% of production fuel, reduce greenhouse gas emissions by about 50%, and reduce asphalt fumes and other harmful gas emissions by more than 80%. DETAILED DESCRIPTION

[0080] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with embodiments.

[0081] Examples 1-3

[0082] A first-stage modified asphalt and preparation method thereof:

[0083] S1 Prepare the first-order modifier and heavy cross-linking asphalt. The mass components of the first-order modifier and heavy cross-linking asphalt are shown in Table 1-2.

[0084] The modifier is obtained by mixing the raw materials according to the ratio of Table 1-1;

[0085] S2 heating the asphalt, the heating temperature is shown in Table 2;

[0086] S3

[0087] S4: adding the first-order modifier to the heated asphalt and mixing. The mixing time is shown in Table 2.

[0088] S5 passes the mixture through an open mill, repeatedly rolling it into sheets, and then shearing it into pieces of 1-5 cm in size by a slitting machine, and grinding it into 200 mesh powder by a liquid nitrogen deep-cooling grinding mill.

[0089] S6 The sheared fragments are crushed by a cryogenic mill to obtain the first-stage modified asphalt; the cryogenic temperature is shown in Table 2

[0090] Embodiment 4-6

[0091] A second-stage modified asphalt and its preparation method: its raw material ratio and process parameters are shown in Table 3 and Table 4 respectively.

[0092] S1 prepares a second-stage modifier, a second-stage modified asphalt, sulfur, and an organosilicon oligomer resin rubber modifier according to the ratios of Table 3 and Table 4;

[0093] S2 The preparation method of the second-stage modifier is: all components are mixed in a reactor, and the heating temperature 1 and the reaction time are shown in Table 5. S3 The first-stage modified asphalt obtained in Examples 1-3 is heated, and the heating temperature 2 is shown in Table 5; Examples 4-6 correspond to the first-stage modified asphalt obtained in Examples 1-3;

[0094] S4: Add the secondary modifier, sulfur, and silicone oligomer resin rubber modifier to the heated asphalt in step 3 and mix. The mixing time is shown in Table 5.

[0095] S5 is obtained by shearing the mixture.

[0096] Embodiment 7-9

[0097] An ultra-thin layer of asphalt and its preparation method:

[0098] S1 prepares raw materials;

[0099] S1-1 Prepare a first-stage modified asphalt according to any one of Examples 1-3;

[0100] S1-2 Prepare a second-stage modified asphalt according to any one of Examples 4-6;

[0101] Example 7 uses the first-stage modified asphalt and the second-stage modified asphalt of Example 1 and Example 4.

[0102] Example 8 uses the first-stage modified asphalt and the second-stage modified asphalt of Example 2 and Example 5,

[0103] Example 9 uses the first-stage modified asphalt and the second-stage modified asphalt of Example 3 and Example 6.

[0104] S1-3 Prepare the raw materials of the active agent according to Table 6;

[0105] The preparation method of S2 active agent is:

[0106] S2-1 polyoxyethylene ether and polyoxypropylene ether are added into the reaction kettle and stirred. The heating temperature is shown in Table 8.

[0107] S2 -2 then add other active agent components and mix in the reactor. The reaction time is shown in Table 8;

[0108] S2 -3 Add distilled water and cool to room temperature

[0109] S3 heats the second-stage modified asphalt, and the heating temperature 2 is shown in Table 8;

[0110] S4: adding the active agent to the second-stage modified asphalt in step 3 and mixing. The mixing time is shown in Table 8;

[0111] S4 is obtained by shearing the mixture.

[0112] Example 10

[0113] A method for constructing an ultra-thin layer of asphalt using the asphalt prepared in Examples 7-9 at low temperature, wherein the thickness of the asphalt concrete to be constructed is 0.7-1.5 cm and the construction temperature is above -5°C.

[0114] Table 1-1 Ratio of raw materials of first-order modifier

[0115]

[0116] Table 1-2 Ratio of raw materials for first-stage modified asphalt

[0117]

[0118] Table 2 Process parameters for preparation of first-stage modified asphalt

[0119]

[0120] Table 3 Secondary modifier raw material ratio

[0121]

[0122] Table 4 Ratio of raw materials for second-stage modified asphalt

[0123]

[0124] Table 5 Process parameters for preparation of second-stage modified asphalt

[0125]

[0126] Table 6 Proportion of raw materials of active agent

[0127]

[0128] Table 7 Raw material ratio of ultra-thin asphalt layer

[0129]

[0130] Table 8 Process parameters for preparing ultra-thin asphalt layer

[0131]

[0132] The main indicators of the heavy traffic asphalt in the embodiment of the present invention are:

[0133] Needle penetration, in units of 0.1 mm: 60-80; according to T 0604-2011 test method; Elongation at 10°C: minimum 20 cm; according to T 0605-2011 test method; Softening point: minimum 46°C; according to T 0606-2011 test method;

[0134] The performance indicators of the asphalt after the first modification are: the asphalt softening point is greater than 80. It can be seen that through the first modification, compared with the existing technology, the needle penetration is reduced by about 16 and the softening point is increased by 20°C.

[0135] The performance indicators of the asphalt after the second modification are: ductility greater than 40. It can be seen that through the second modification, compared with the first-order modified asphalt, the ductility is increased and the viscosity is reduced.

[0136] The performance indicators of the final asphalt obtained after the third modification are as follows:

[0137]

[0138] It can be seen that through the third modification, an ultra-thin layer of asphalt suitable for low-temperature construction with high fluidity, high softening point, high ductility and high toughness is obtained. This asphalt has the following advantages:

[0139] 1. Good stability, easy for long-term storage, transportation and use.

[0140] 2. The softening point after aging is greater than 70, and the elongation is greater than 40. That is, the high temperature resistance in summer and the crack resistance in winter are balanced.

[0141] 3. It can effectively prevent and delay reflective cracks.

[0142] 4. The high-viscosity and high-elastic asphalt after aging has good fluidity before paving, and the kinematic viscosity at 100°C is less than 3.

[0143] 5. No special equipment is required for paving, any ordinary paver can be used.

[0144] 6. It can effectively reduce asphalt smoke emissions by more than 50%, and the discharge temperature of the ultra-thin mixture can be 135-145℃.

[0145] 7. The operating temperature of asphalt is lower. The ultra-thin layer of asphalt produced by low-temperature construction technology has very good fluidity at 110-120 degrees Celsius.

[0146] 8. The indicators after aging are easier to ensure the forming stability and quality stability of ultra-thin layers with a thickness of 1-1.5cm.

[0147] The ultra-thin layer of low-temperature construction technology generally refers to a functional layer of asphalt surface layer with a thickness of asphalt concrete between 0.7-1.5. It is mainly used to repair the roughness, rutting, and cracking of asphalt pavement and to convert old cement pavement from white to black, etc. The construction temperature is above -5℃ and there is no water accumulation on the road surface, so construction and paving can be carried out.

[0148] The ultra-thin modified asphalt of the present invention has good fluidity of the mixture, and the paving temperature requires that the ultra-thin mixture be 100°C. The rolling temperature requirement is low, and the initial pressure of the ultra-thin mixture is above 70 degrees, and the final pressure of the ultra-thin mixture is above 50 degrees. No special synchronous paver is required, and ordinary domestic brands of pavers can be used for construction. The problems of high seasonal restrictions on construction and high equipment requirements due to material problems are greatly reduced. By optimizing the modified materials and processes, its performance is greatly optimized to meet the requirements of open construction conditions, so that it should be applied in a wider range of scenarios. It is suitable for rapid repair of local diseases of the original road surface, and can strengthen the interlayer bonding strength. By adding a 1-1.5cm warm-mixed ultra-thin wear layer, the flatness, structural depth, anti-skid performance, and road appearance of the original road surface are restored and improved, extending the service life of the road surface, improving the driving comfort and safety of the road surface, and reducing driving noise. It meets the strategic needs and positioning of the national transportation power strategy for lightweight, intensive, and green pre-maintenance technology.

[0149] The above is only an embodiment of the present invention. The common sense such as the known specific structure and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field are aware of all the common technical knowledge in the technical field of the invention before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement the scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for the ordinary technicians in the relevant field to implement this application. It should be pointed out that for the technicians in this field, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A first-stage modified asphalt, characterized in that: The asphalt is composed of the following mass components: 85-90 parts of base asphalt 10-15 parts of first-stage modifier The first-order modifier is composed of the following mass components: 5-8 parts rock asphalt SBS 65 parts SBR 20-25 parts 5-7 parts tung oil The base asphalt is heated to between 140-160°C, a first-order modifier is added and mixed, the mixture is sheeted and sheared, and then deep-cold and ground into powder by liquid nitrogen to obtain a first-order modified asphalt.

2. A second-stage modified asphalt, characterized in that: The asphalt is composed of the following mass components: First-stage modified asphalt 86.5-91.5 parts Sulfur: 0.5 parts Silicone oligomer: 3-8 parts Second stage modifier: 5 parts The second-stage modifier is composed of the following mass components: 25-30 parts of tung oil Epoxidized soybean oil 8-12 parts Phthalic anhydride 20-30 parts Pentaerythritol 12-20 parts 3-6 parts of glycerol 3-5 parts of C9 petroleum resin C5 petroleum resin 5-7 parts C10 petroleum resin 6-8 parts 2-4 parts of acrylic acid 2-4 parts of resin catalyst; The components for preparing the second-stage modifier are heated to 120-160°C in a reactor for 6-10 hours to obtain the second-stage modifier; the first-stage asphalt is heated to between 140-160°C, sulfur, silicone oligomer and second-stage modifier are added, and the mixture is sheared to obtain the product.

3. An ultra-thin layer of asphalt, characterized in that: The asphalt is composed of the following mass components: Second stage modified asphalt 92-95 parts Active agent 5-8 parts The active agent is composed of the following mass components: The components for preparing the activator are added into a reaction kettle, mixed and stirred to obtain the activator; the second-stage modified asphalt is heated to between 140-160° C., the activator is added, and the mixture is sheared to obtain the activator.

4. The asphalt according to claim 1, characterized in that: Therefore, the particle size of the first-order modified asphalt is 100-300 mesh.

5. The asphalt according to claim 4, characterized in that: The particle size of the first-order modified asphalt is 200 meshes.

6. A method for preparing an ultra-thin layer of asphalt, characterized in that: The following steps are involved: S1. Preparation of a first-order modifier: uniformly mix the following raw materials by mass, including 5-8 parts of rock asphalt, 65 parts of SBS, 20-25 parts of SBR, and 5-7 parts of tung oil; S2. Heat the base asphalt to 140-160°C, add the first-order modifier, and mix for 0.5-1h; wherein the base asphalt is 85-90 parts and the first-order modifier is 10-15 parts; S3, the mixture is pressed, sheared and crushed in sequence to obtain the first-order modified asphalt S4, preparation of the second-order modifier: adding the following raw materials by mass into the reactor, 25-30 parts of tung oil, 8-12 parts of epoxidized soybean oil, 20-30 parts of phthalic anhydride, 12-20 parts of pentaerythritol, 3-6 parts of glycerol, 3-5 parts of C9 petroleum resin, 5-7 parts of C5 petroleum resin, 6-8 parts of C10 petroleum resin, 2-4 parts of acrylic acid, 2-4 parts of resin catalyst; heating temperature 120-160°C, reaction time 6-10h; S5. Heat the first-stage modified asphalt to 140-160°C, add the second-stage modifier, sulfur, and silicone oligomer resin rubber modifier, and mix for 0.5-1h; wherein the first-stage modified asphalt is 86.5-91.5 parts, the second-stage modifier is 5 parts, the sulfur is 0.5 parts, and the silicone oligomer resin rubber modifier is 3-8 parts; S6, shearing the mixture to obtain a second-stage modified asphalt; S7, prepare active agent: mix the raw materials of the following mass components; add 20 parts of polyoxyethylene ether and 30 parts of polyoxypropylene ether into the reaction kettle and stir, and heat to 50°C-80°C; then add 0.02 parts of dibutyltin dilaurate, 20 parts of anthracene epoxy modified silicone oil, 3 parts of toluene diisocyanate, and 10 parts of hexamethylene diisocyanate, mix and stir for 0.5h-1h; then add 16.98 of distilled water and cool to room temperature; S8. Heat the second-stage modified asphalt to 140-160°C, add the active agent and mix for 0.5-1h; S9. Shear the mixture to obtain an extremely thin layer of asphalt.

7. A method of using the ultra-thin layer of asphalt described in claim 6 for low-temperature construction, characterized in that: The thickness of the asphalt concrete under construction is 0.7-1.5cm, and the construction temperature is above minus 5℃.