Functional water-based paint and preparation method thereof
A functionalized water-based coating with specific components forms a stable network structure to address compatibility issues, maintaining antibacterial and mildew-proof capabilities, enhancing long-term resistance and weather resistance.
Patent Information
- Application Number
- CN202411217565.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Existing water-based acrylic resin coatings suffer from compatibility issues with organic fungicides, leading to rapid loss and decline in antibacterial ability and weather resistance, resulting in poor long-term mildew resistance and outdoor performance.
A functionalized water-based coating comprising specific ratios of water-based acrylic resin, alkyd resin, hexamethoxymethyl melamine, silane coupling agent, film-forming aid, composite fungicide, and stabilizer, which forms a stable network structure to maintain antibacterial and mildew-proof capabilities over time.
The coating achieves excellent antibacterial and anti-mildew functions with high stability and strong weather resistance, reducing fungicide loss and migration, ensuring long-term effectiveness outdoors.
Smart Images

Figure CN119060591A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional coatings, in particular to the technical field of water-based acrylic resin coatings with long-term mildew resistance. Background Art
[0002] During the production process of water-based paint, a large amount of water, cellulose, organic resin emulsion and other organic substances are added, which provides suitable growth conditions and nutrients for microorganisms such as bacteria and algae. As a result, under certain environmental conditions, various molds and bacteria can easily multiply in large numbers on the coating film, causing erosion of the paint film, seriously affecting the weather resistance of the water-based resin coating.
[0003] In order to improve the mildew resistance of water-based paint, a feasible technical means is to add additives with bactericidal effects to water-based paint, especially to add organic fungicides for compatibility with the organic system of water-based paint. However, it is found in practice that if organic fungicides with good bactericidal effects are directly added to the water-based paint system, not only will there still be certain compatibility issues between the two, but also, over time, the organic fungicides will continue to be lost in the water-based paint and the coating formed by it, resulting in the continuous weakening of the antibacterial ability of the paint and the rapid decline of the coating performance. In addition, the water-based paint after adding organic fungicides often has certain other performance losses, resulting in a significant decline in weather resistance when used outdoors.
[0004] Therefore, obtaining a water-based acrylic resin coating with long-term mildew resistance and always maintaining excellent weather resistance is still a technical problem to be solved in the prior art. Summary of the invention
[0005] In order to solve the above-mentioned problems of the prior art, the object of the present invention is to provide a functionalized water-based coating and a preparation method thereof which can stably maintain excellent antibacterial and mildew-proof capabilities for a long time and has excellent outdoor weather resistance.
[0006] The technical solution of the present invention is as follows:
[0007] A functionalized water-based coating comprises the following raw material components in parts by weight: 75.00-90.00 parts of a water-based acrylic resin, 1.00-8.00 parts of an alkyd resin, 2.00-8.00 parts of hexamethoxymethyl melamine (HMMM) and / or 2.00-8.00 parts of a silane coupling agent 3-aminopropyl triethoxysilane (KH550), 1.00-3.00 parts of a film-forming aid dipropylene glycol butyl ether (DPNB), 1.00-3.00 parts of a composite fungicide and 5.00-15.00 parts of water, wherein the composite The fungicide comprises the following raw material components in parts by mass: 3.80-9.20 parts of isothiazolinone organic mildew preventer, 2.00-8.10 parts of metconazole organic mildew preventer, 2.50-8.00 parts of iodopropynyl n-butylcarbamate (IPBC), 1.20-6.00 parts of 4-bromo-2,5-dichlorophenol (DP), 12.00-25.00 parts of 4-tolyldiiodomethyl sulfone, 25.00-35.00 parts of benzyl alcohol, 12.00-30.00 parts of surfactant and 10.00-20.00 parts of stabilizer.
[0008] Preferably, the functionalized water-based coating comprises the following raw material components in parts by mass: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of hexamethoxymethyl melamine (HMMM), 1.50-2.60 parts of film-forming aid dipropylene glycol butyl ether (DPNB), 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water, wherein the composite fungicide comprises the following raw material components in parts by mass: .00-8.60 parts of isothiazolinone organic mildew preventer, 2.60-5.60 parts of metconazole organic mildew preventer, 4.00-6.40 parts of iodopropynyl n-butylcarbamate (IPBC), 13.00-20.00 parts of 4-tolyldiiodomethyl sulfone, 1.65-4.00 parts of 4-bromo-2,5-dichlorophenol (DP), 30.00-35.00 parts of benzyl alcohol, 15.00-30.00 parts of surfactant and 10.00-15.00 parts of stabilizer.
[0009] Or, preferably, the functionalized water-based coating comprises the following raw material components in parts by mass: the functionalized water-based coating according to claim 1, characterized in that it comprises the following raw material components in parts by mass: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of silane coupling agent 3-aminopropyltriethoxysilane (KH550), 1.80-2.40 parts of film-forming aid dipropylene glycol butyl ether (DPNB), 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water, wherein The composite fungicide comprises the following raw material components in parts by mass: 4.50-7.50 parts of isothiazolinone organic mildew inhibitor, 2.80-6.20 parts of metconazole organic mildew inhibitor, 3.00-6.40 parts of iodopropynyl n-butylcarbamate (IPBC), 14.00-20.00 parts of 4-tolyldiiodomethyl sulfone, 2.00-4.00 parts of 4-bromo-2,5-dichlorophenol (DP), 25.00-35.00 parts of benzyl alcohol, 14.00-20.00 parts of surfactant and 12.00-20.00 parts of stabilizer.
[0010] Or, preferably, the functionalized water-based coating comprises the following raw material components in parts by mass: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of hexamethoxymethyl melamine (HMMM) or 3.00-5.00 parts of silane coupling agent 3-aminopropyl triethoxysilane (KH550), 1.50-2.20 parts of film-forming aid dipropylene glycol butyl ether (DPNB), 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water The composite fungicide comprises the following raw material components in parts by mass: 5.20-8.00 parts of isothiazolinone organic mildew inhibitor, 2.20-4.20 parts of metconazole organic mildew inhibitor, 3.00-4.60 parts of iodopropynyl n-butylcarbamate (IPBC), 12.00-16.00 parts of 4-tolyl diiodomethyl sulfone, 1.80-3.20 parts of 4-bromo-2,5-dichlorophenol (DP), 25.00-30.00 parts of benzyl alcohol, 15.00-25.00 parts of surfactant and 10.00-20.00 parts of stabilizer.
[0011] Preferably, the water-based acrylic resin has a molecular weight of 10,000-12,000 and / or a viscosity of 250 mPa·s-300 mPa·s.
[0012] More preferably, the water-based acrylic resin has a molecular weight of 10,000, a viscosity of 250 mPa·s, a solid content of 50%, and a pH of 8.
[0013] Preferably, the hydroxyl value of the alkyd resin is 12-15 mgKOH / g.
[0014] More preferably, the alkyd resin has a solid content of 40% and a hydroxyl value (mgKOH / g) of 12.
[0015] The present invention further provides a method for preparing the functionalized water-based coating, which comprises: first mixing the water-based acrylic resin, the alkyd resin, the hexamethoxymethyl melamine and / or the silane coupling agent 3-aminopropyl triethoxysilane (KH550), the film-forming aid dipropylene glycol butyl ether (DPNB), and the water under the action of mechanical force, then adding the composite fungicide, and performing a second mixing under the action of mechanical force to obtain the functionalized water-based coating.
[0016] Preferably, the first mixing condition is stirring at a temperature of 30-40° C. and a rotation speed of 400-800 rpm for 20-30 min.
[0017] Preferably, the second mixing condition is stirring at a temperature of 40-50° C. and a rotation speed of 200-600 rpm for 10-20 min.
[0018] The functionalized water-based coating of the present invention has excellent antibacterial and anti-mildew functions, high stability, strong anti-loss and strong weather resistance, and can be used outdoors for a long time;
[0019] The functionalized water-based coating of the present invention can reduce the loss, migration and degradation of the fungicide during use through the cross-linking effect of the modified acrylic resin system and the composite fungicide, thereby improving the long-term mildew resistance and weather resistance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a comparison chart of the results of the mixed mold and mildew prevention test in the examples.
[0021] Figure 2 This is a comparison chart of aging results when performing weathering tests in the embodiments.
[0022] Figure 3 This is a comparison chart of the Aspergillus niger mildew resistance test results when performing the runoff test in the examples. DETAILED DESCRIPTION
[0023] The technical scheme of the present invention will be further described below in conjunction with the embodiments and drawings of the present invention. The embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0024] The surfactant used in the following examples may be one or more of sodium dialkyl sulfate (SDS), sodium lauryl polyoxyethylene ether sulfate (AES), cocamidopropyl betaine (CAPB), dodecyltrimethylammonium chloride (DTAC), fatty alcohol polyoxyethylene ether (AEO), alkylphenol polyoxyethylene ether (OP), cocamidopropyl dimethylaminoethyl lactone (CAB), lauryl amide propyl dimethylaminoethyl lactone (LAB), etc.; the stabilizer may be one or more of sodium silicate (salt), polyacrylamide, isopropyl phosphate, polyvinyl alcohol, magnesium nitrate, etc.; the isothiazolinone organic mildew inhibitor may be selected from one or more of octyl isothiazolinone (OIT), dichloro-N-octyl-4-isothiazolinone (DCOIT) and benzisothiazolinone (BIT), etc.
[0025] The aqueous acrylic resin used in the following examples has a molecular weight of 10,000, a viscosity of 250 mPa·s, a solid content of 50%, and a pH of 8. The alkyd resin used has a solid content of 40% and a hydroxyl value (mgKOH / g) of 12.
[0026] Example 1
[0027] 78.00 g of waterborne acrylic resin, 2.00 g of alkyd resin, 4.00 g of hexamethoxymethyl melamine (HMMM), 2.00 g of film-forming aid dipropylene glycol butyl ether (DPNB) and 12.00 g of water were mixed and stirred at 40°C and 500 rpm for 20-30 min, then 2.00 g of composite fungicide TCB was added thereto and stirred at 50°C and 400 rpm for another 15 min. min, to prepare the functionalized water-based coating of the present invention; wherein the composite fungicide TCB is composed of: 6.70 parts of isothiazolinone organic mildew inhibitor, 3.60 parts of metconazole organic mildew inhibitor, 4.00 parts of iodopropynyl n-butylcarbamate (IPBC), 15.00 parts of 4-tolyl diiodomethyl sulfone, 4.00 parts of 4-bromo-2,5-dichlorophenol (DP), 30.00 parts of benzyl alcohol, 20.00 parts of surfactant and 15.00 parts of stabilizer.
[0028] Example 2
[0029] 82.00 g of water-based acrylic resin, 3.00 g of alkyd resin, 3.00 g of HMMM, 2.60 g of DPNB and 9.00 g of water were mixed, and stirred at a temperature of 40° C. and a rotation speed of 500 rpm for 30 min, and then 2.00 g of composite fungicide ADZ was added thereto, and stirred at a temperature of 50° C. and a rotation speed of 400 rpm for another 15 min to obtain the functionalized water-based coating of the present invention; wherein the composite fungicide ADZ is composed of: 7.50 parts of isothiazolinone organic mildew inhibitor, 4.20 parts of metconazole organic mildew inhibitor, 3.40 parts of IPBC, 20.00 parts of 4-tolyl diiodomethyl sulfone, 3.40 parts of DP, 30.00 parts of benzyl alcohol, 15 parts of surfactant and 15.00 parts of
[0030] Stabilizer.
[0031] Example 3
[0032] 85g.00 water-based acrylic resin, 2.00g alkyd resin, 4.00g HMMM, 1.80g DPNB and 13.00g water are mixed and stirred at a temperature of 40°C and a rotation speed of 500rpm for 30min, and then 2.00g composite fungicide NDA is added thereto, and stirred for another 15min at a temperature of 50°C and a rotation speed of 400rpm to prepare the functionalized water-based coating of the present invention; wherein the composite fungicide NDA is composed of: 8.50 parts of isothiazolinone organic mildew inhibitor, 5.20 parts of metconazole organic mildew inhibitor, 5.20 parts of IPBC, 12.00 parts of 4-tolyl diiodomethyl sulfone, 2.80 parts of DP, 35.00 parts of benzyl alcohol, 20.00 parts of surfactant and 15.00 parts of stabilizer.
[0033] Example 4
[0034] 90.00g of waterborne acrylic resin, 4.00g of alkyd resin, 4.00g of KH550, 1.50g of DPNB and 8.00g of water are mixed, and stirred at a temperature of 40°C and a rotation speed of 500rpm for 30min, and then 3.00g of composite fungicide NDA is added thereto, and stirred at a temperature of 50°C and a rotation speed of 400rpm for another 15min to prepare the functionalized waterborne coating of the present invention; wherein the composite fungicide NDA is composed of: 8.50 parts of isothiazolinone organic mildew inhibitor, 5.20 parts of metconazole organic mildew inhibitor, 5.20 parts of IPBC, 12.00 parts of 4-tolyl diiodomethyl sulfone, 2.80 parts of DP, 35.00 parts of benzyl alcohol, 20.00 parts of surfactant and 15.00 parts of stabilizer.
[0035] Example 5
[0036] 88.00g of water-based acrylic resin, 3.00g of alkyd resin, 4.00g of KH550, 1.60g of DPNB and 12.00g of water are mixed, and stirred at a temperature of 35°C and a rotation speed of 500rpm for 30min, and then 2.00g of composite fungicide TCB is added thereto, and stirred at a temperature of 50°C and a rotation speed of 400rpm for another 15min to prepare the functionalized water-based coating of the present invention; wherein the composite fungicide TCB is composed of: 6.70 parts of isothiazolinone organic mildew inhibitor, 3.60 parts of metconazole organic mildew inhibitor, 4.00 parts of IPBC, 15.00 parts of 4-tolyl diiodomethyl sulfone, 4.00 parts of DP, 30.00 parts of benzyl alcohol, 20.00 parts of surfactant and 15.00 parts of stabilizer.
[0037] Example 6
[0038] 82.00g of water-based acrylic resin, 1.00g of alkyd resin, 3.00g of KH550, 2.00g of DPNB and 15.00g of water were mixed, and stirred at a temperature of 35°C and a rotation speed of 500rpm for 30min, and then 3g of composite fungicide ADZ was added thereto, and stirred at a temperature of 45°C and a rotation speed of 400rpm for another 15min to prepare the functionalized water-based coating of the present invention; wherein the composite fungicide ADZ is composed of: 7.50 parts of isothiazolinone organic mildew inhibitor, 4.20 parts of metconazole organic mildew inhibitor, 3.40 parts of IPBC, 20 parts of 4-tolyl diiodomethyl sulfone, 3.40 parts of DP, 30.00 parts of benzyl alcohol, 15 parts of surfactant and 15.00 parts of stabilizer.
[0039] Comparative Example 1
[0040] Untreated bamboo.
[0041] Comparative Example 2
[0042] 90.00 g of waterborne acrylic resin, 2.00 g of alkyd resin, 4.00 g of HMMM and 9.00 g of water were mixed and stirred at 35° C. and 400 rpm for 15 min to prepare a waterborne coating.
[0043] Comparative Example 3
[0044] 88.00 g of water-based acrylic resin, 2.00 g of composite fungicide ADZ, 2.00 g of DPNB and 8.00 g of deionized water were stirred at 40° C. and 400 rpm for 15 min to prepare a water-based antibacterial coating, wherein the composite fungicide ADZ was composed of 7.50 parts of isothiazolinone organic mildew inhibitor, 4.20 parts of metconazole organic mildew inhibitor, 3.40 parts of IPBC, 20 parts of 4-tolyldiiodomethyl sulfone, 3.40 parts of DP, 30.00 parts of benzyl alcohol, 15.00 parts of a surfactant and 15.00 parts of a stabilizer.
[0045] Comparative Example 4
[0046] 80.00 g of water-based acrylic resin, 4.00 g of HMMM and 9.00 g of water were mixed and stirred at 35° C. and 500 rpm for 30 min, and then 2.00 g of propiconazole was added thereto, and stirred at 40° C. and 400 rpm for further 15 min to prepare a water-based antibacterial coating.
[0047] Comparative Example 5
[0048] 80.00 g of water-based acrylic resin, 2.00 g of alkyd resin, 4.00 g of HMMM, 1.50 g of DPNB and 9.00 g of water were mixed and stirred at 30° C. and 500 rpm for 30 min. Subsequently, 2.00 g of propiconazole was added thereto and stirred at 40° C. and 400 rpm for 15 min to prepare a water-based antibacterial coating.
[0049] Comparative Example 6
[0050] 82.00 g of water-based acrylic resin, 2.00 g of alkyd resin and 9.00 g of water were mixed, and stirred at a temperature of 35° C. and a rotation speed of 500 rpm for 30 min. 3.00 g of a comparative fungicide was added to the water-based acrylic resin coating, and stirred at a temperature of 40° C. and a rotation speed of 400 rpm for 15 min to prepare a water-based antibacterial coating; wherein the comparative fungicide was composed of: 8.70 parts of IPBC, 15.00 parts of 4-tolyldiiodomethyl sulfone, 30.00 parts of benzyl alcohol, 20.00 parts of a surfactant and 24.00 parts of a stabilizer.
[0051] The coatings obtained in Examples 1, 2, 5 and Comparative Examples 2 and 4 were applied to bamboo specimens, each specimen was applied twice, and after drying for 24 hours at 25°C, a mixed multi-bacteria environment mildew resistance test was performed with reference to GB / T 18261-2000 "Test Method for Control of Wood Mold and Blue Stain Fungi by Mildew Inhibitors" and American Wood Protection Association Standard AWPA E24-06, and the same bamboo specimen (Comparative Example 1) not coated with the coating was used as a comparison. The control efficacy was calculated according to the following formula in the test:
[0052]
[0053] Where: RE is the control effect, D t is the average damage value of the specimen; D o is the average damage value of the control sample. The results are shown in Table 1 and Appendix Figure 1 As shown, Figure 1 a is the bamboo specimens before painting, 1b is the bamboo specimens after painting for 14 weeks.
[0054] Table 1 Test results of bamboo anti-mildew performance
[0055] Test piece Mixed mold control effectiveness Victim value Example 1 100 0 Example 2 100 0 Example 5 100 0 Comparative Example 2 0 4 Comparative Example 4 25 3 Untreated bamboo 0 4
[0056] According to the above test results, it can be seen that the infection value of untreated bamboo is as high as 4 after 14 weeks, while the bamboo (Examples 1, 2, and 5) using the functionalized water-based coating of the present invention has a damage value of 0 under the same conditions, and the anti-mildew effect can be as high as 100%. The bamboo (Comparative Example 4) of the system of ordinary fungicide and modified acrylic resin compound has a damage value of 3 and a control effect of 25%, which shows that the modified coating under the ordinary compounding system alone does not have an excellent long-term anti-mildew effect, and the functionalized coating of the composite system of the present invention has an excellent anti-mildew effect and is long-lasting.
[0057] Furthermore, the functionalized water-based coatings obtained in Examples 1, 3, 4, 5, and 6, and the fungicides or coatings obtained in Comparative Examples 3 and 5 were applied to bamboo specimens. Each specimen was applied twice. After drying for 24 hours at 25°C, an aging test was carried out in a fluorescent ultraviolet aging test chamber. The same bamboo specimens that were not coated with the coating were used as a comparison.
[0058] In the aging test, the lamps in the box are UVB-340 lamps that can simulate short-wave ultraviolet light. The ambient temperature is 50°C. Water is sprayed once every 102 minutes for 18 minutes. The aging time is 216 hours. The coating aging grade is evaluated by referring to the visual colorimetry of GB / T9761 paint and varnish paint.
[0059] The test results are as attached Figure 2As shown in Table 2. The results show that the aging grade of the untreated bamboo in Comparative Example 1 is 5, and the aging grades of Comparative Examples 3 and 5 are 4, indicating that the coating of the bamboo using only the unmodified water-based acrylic resin and the composite fungicide compounded coating and the coating using only the common fungicide and the modified acrylic resin compounded coating in the composite system has a high degree of aging and poor weather resistance. The aging degree of the coating of the bamboo using the functionalized water-based coating of the present invention as in Examples 1, 3, 4, 5, and 6 is only 0 and 1, indicating that a more compact network structure can be formed between the composite fungicide and the modified water-based acrylic resin in the present invention, which increases the mechanical properties and water resistance of the paint film, thereby making the coating less likely to be damaged, and further increasing the weather resistance of the coating.
[0060] Table 2 Test results of weather resistance of bamboo
[0061] Test piece Degree of change in damage Degree of change Example 1 0 No change, no perceptible change Example 3 1 Very slight, barely noticeable change Example 4 0 No change, no perceptible change Example 5 1 Very slight, barely noticeable change Example 6 0 No change, no perceptible change Comparative Example 3 4 Larger, i.e., greater changes Comparative Example 5 4 Larger, i.e., greater changes Untreated bamboo 5 Severe, i.e. strong changes
[0062] Furthermore, the functionalized water-based coatings of Examples 1, 3, 5, and 6, and the water-based antibacterial coatings of Comparative Example 5 and Comparative Example 6 were applied to bamboo specimens, each specimen was applied twice, and after drying for 24 hours at 25°C, the treated specimens were placed in a beaker, added with water, and placed on a magnetic stirrer for loss at 400 r / min. The water was changed every 6 hours, 12 hours, 18 hours, 24 hours, and 48 hours, and then every 48 hours until 336 hours. After the end, the specimens were taken out, and then the specimens were taken out after 14 days of loss, and a mildew resistance test was carried out on a culture medium full of Aspergillus niger.
[0063] The results of the mildew test after 2 weeks are as follows: Figure 3 As shown, it can be seen from the figure that comparative example 5 is the mildew prevention situation after the loss of the compound system with the addition of fungicide propiconazole and modified acrylic resin, and the prevention and control efficiency is 0%, which proves that the compatibility of ordinary fungicides and modified water-based acrylic resins is poor, and the fungicides have obvious loss and migration. Comparative example 6 is the mildew prevention test result of the ordinary compound system, and its prevention and control efficiency is 25%, which proves that the simple compound system cannot significantly reduce the migration of fungicides during the loss process. The prevention and control efficiency of the fungicides ADZ, NDA, TCB in the present invention after compounding with modified water-based acrylic resin and other additives and stabilizers reaches 100%, which is significantly better than the comparative example, indicating that the compound system of the present invention can significantly reduce the loss and migration of fungicides.
[0064] It should be noted that the above is only a preferred embodiment of the present invention, which should not limit the protection scope of the technical solution of the present invention. Any modification of the technical solution recorded in the above embodiments and equivalent replacement of technical features by ordinary technicians in the field within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A functionalized water-based coating, comprising the following raw material components in parts by mass: 75.00-90.00 parts of water-based acrylic resin, 1.00-8.00 parts of alkyd resin, 2.00-8.00 parts of hexamethoxymethyl melamine and / or 2.00-8.00 parts of 3-aminopropyl triethoxysilane, 1.00-3.00 parts of dipropylene glycol butyl ether, 1.00-3.00 parts of composite fungicide and 5.00-15.00 parts of water, wherein: The composite fungicide comprises the following raw material components in parts by weight: 3.80-9.20 parts of isothiazolinone organic mildew inhibitor, 2.00-8.10 parts of metconazole organic mildew inhibitor, 2.50-8.00 parts of iodopropynyl n-butyl carbamate, 1.20-6.00 parts of 4-bromo-2,5-dichlorophenol, 12.00-25.00 parts of 4-tolyl diiodomethyl sulfone, 25.00-35.00 parts of benzyl alcohol, 12.00-30.00 parts of surfactant and 10.00-20.00 parts of stabilizer.
2. The functionalized water-based coating according to claim 1, characterized in that: The composite fungicide comprises the following raw material components in parts by weight: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of hexamethoxymethyl melamine, 1.50-2.60 parts of dipropylene glycol butyl ether, 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water, wherein the composite fungicide comprises the following raw material components in parts by weight: 4.00-8.60 parts of Isothiazolinone organic mildew preventer, 2.60-5.60 parts of metconazole organic mildew preventer, 4.00-6.40 parts of iodopropynyl n-butyl carbamate, 13.00-20.00 parts of 4-tolyl diiodomethyl sulfone, 1.65-4.00 parts of 4-bromo-2,5-dichlorophenol, 30.00-35.00 parts of benzyl alcohol, 15.00-30.00 parts of surfactant and 10.00-15.00 parts of stabilizer.
3. The functionalized water-based coating according to claim 1, characterized in that: It includes the following raw material components in parts by mass: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of 3-aminopropyl triethoxysilane, 1.80-2.40 parts of dipropylene glycol butyl ether, 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water, wherein the composite fungicide includes the following raw material components in parts by mass: 4.50-7.50 parts Isothiazolinone organic mildew preventer, 2.80-6.20 parts of metconazole organic mildew preventer, 3.00-6.40 parts of iodopropynyl n-butyl carbamate, 14.00-20.00 parts of 4-tolyl diiodomethyl sulfone, 2.00-4.00 parts of 4-bromo-2,5-dichlorophenol, 25.00-35.00 parts of benzyl alcohol, 14.00-20.00 parts of surfactant and 12.00-20.00 parts of stabilizer.
4. The functionalized water-based coating according to claim 1, characterized in that: The composite fungicide comprises the following raw material components in parts by weight: 80.00-90.00 parts of water-based acrylic resin, 1.00-3.00 parts of alkyd resin, 3.00-5.00 parts of hexamethoxymethyl melamine or 3.00-5.00 parts of 3-aminopropyl triethoxysilane, 1.50-2.20 parts of film-forming aid dipropylene glycol butyl ether, 1.00-3.00 parts of composite fungicide and 8.00-10.00 parts of water, wherein the composite fungicide comprises the following raw materials in parts by weight: Components: 5.20-8.00 parts of isothiazolinone organic mildew preventer, 2.20-4.20 parts of metconazole organic mildew preventer, 3.00-4.60 parts of iodopropynyl n-butyl carbamate, 12.00-16.00 parts of 4-tolyl diiodomethyl sulfone, 1.80-3.20 parts of 4-bromo-2,5-dichlorophenol, 25.00-30.00 parts of benzyl alcohol, 15.00-25.00 parts of surfactant and 10.00-20.00 parts of stabilizer.
5. The functionalized water-based coating according to claim 1, characterized in that: The water-based acrylic resin has a molecular weight of 10,000-12,000 and / or a viscosity of 250 mPa·s-300 mPa·s.
6. The functionalized water-based coating according to claim 1, characterized in that: The hydroxyl value of the alkyd resin is 12-15 mgKOH / g.
7. The method for preparing the functionalized water-based coating according to any one of claims 1 to 4, characterized in that: It includes: The water-based acrylic resin, the alkyd resin, the hexamethoxymethyl melamine and / or 3-aminopropyl triethoxysilane, the dipropylene glycol butyl ether and the water are first mixed under the action of mechanical force, and then the composite fungicide is added and secondly mixed under the action of mechanical force to obtain the functionalized water-based coating.
8. The preparation method according to claim 7, characterized in that: The first mixing condition is stirring at a temperature of 30-40° C. and a rotation speed of 400-800 rpm for 20-30 min.
9. The preparation method according to claim 7, characterized in that: The second mixing condition is stirring at a temperature of 40-50° C. and a rotation speed of 200-600 rpm for 10-20 min.
Citation Information
Patent Citations
Biocidal agent
CN106163282A
Water-based mildew-proof environment-friendly coating material and preparation method thereof
CN112375479A
Colorless water-borne multifunctional wood preservative as well as preparation and use methods thereof
CN113199579A
High-temperature-resistant water-borne wood and bamboo organic mildew inhibitor and preparation method thereof
CN114766497A
Wood preservative, esp. for fungus and insect control
DE4406819A1
Cited By
Water-based weather-resistant mildew-proof coating as well as preparation method and application thereof
CN120005457A