High-adhesion free radical curing UV metal printing gloss oil and preparation method thereof

By using modified epoxy acrylate resin, polyester acrylate and amino acrylate to form a tight network structure, the problem of poor adhesion of free radical cured UV iron polish is solved, and high adhesion and stable processing performance are achieved , meets the requirements of complex production environments.

CN119060619APending Publication Date: 2024-12-03SHANGHAI YUCAI PACKAGING MATERIAL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411364077.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The poor adhesion of radically cured UV printing irradiated oil leads to insufficient binding force with substrates such as white codine and ink, which cannot meet the production and processing requirements.

Method used

Modified epoxy acrylate resin, polyester acrylate and amino acrylate are used as radical curing oligomers and monomers, combining specific initiators and adhesion accelerators to form a tight network structure, reducing volume shrinkage and improving Adhesion.

Benefits of technology

It significantly improves the adhesion between UV iron polish and the substrate, reduces the volume shrinkage rate of the cured film, avoids cracks and peeling problems, meets the requirements of the complex production and processing environment, and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005065706310000051
    Figure BDA0005065706310000051
  • Figure BDA0005065706310000061
    Figure BDA0005065706310000061
Patent Text Reader

Abstract

The invention provides high-adhesion free radical curing UV metal printing gloss oil and a preparation method thereof, and relates to the technical field of gloss oil. The high-adhesion free radical curing UV metal printing gloss oil is prepared from the following components in parts by weight: 45 to 65 parts of free radical curing oligomer, 25 to 44 parts of free radical curing monomer, 2 to 4 parts of free radical initiator, 6 to 10 parts of adhesion promoter, 0.05 to 0.5 part of flatting agent and 0.05 to 0.5 part of defoaming agent. The preparation method comprises the following steps: mixing and uniformly stirring the free radical curing oligomer, the free radical curing monomer and the adhesion promoter; adding a free radical initiator into the mixture and stirring; and adding the flatting agent and the defoaming agent into the mixture, and stirring to obtain the paint. By selecting the proper free radical curing oligomer and free radical curing monomer, the gloss oil is ensured to have excellent film-forming property and physical property while being rapidly cured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of varnishes, and in particular to a high-adhesion free radical-cured UV iron printing varnish and a preparation method thereof. Background Art

[0002] Tinplate, as the main material of the metal packaging industry, has a very broad market base. It is most widely used in canning packaging, high-quality packaging, and chemical product packaging. The coating process of these products is as follows: surface treatment of tinplate, coating with white primer, printing with color ink, and applying varnish. Among them, varnish is the outermost coating, usually composed of resin and additives, and the paint film is shiny after curing.

[0003] Varnish is mainly divided into traditional solvent-based varnish and new UV curing varnish. At present, most domestic manufacturers use traditional solvent-based varnish, which contains 40%-60% volatile organic solvents. When used, it must go through a high-temperature baking process of 10-20 minutes to volatilize the solvent and cross-link and cure to obtain a qualified varnish coating. The production workshop has high temperature and strong odor. The baked solvent must also be treated in an RTO incinerator, further increasing energy consumption. The high production cost also affects the physical and mental health of workers. In order to balance economic benefits and environmental protection, the transformation of traditional solvent-based varnish is imperative.

[0004] The new UV curing varnish is cured by ultraviolet lamp. The solid content in the system is high, the curing time is short, and no volatile solvent is produced. Therefore, it can greatly improve the production efficiency and environmental performance of tinplate varnish. UV curing technology is divided into two mechanisms: free radical curing and cationic curing. Compared with cationic curing, free radical curing has the advantages of fast curing speed, a wide variety of resins and monomers, and low price. Therefore, the practical application value of free radical curing is extremely high. However, the volume shrinkage rate of free radical curing is high, which easily leads to poor adhesion between it and white cotin and ink, and cannot meet the production and processing requirements. Summary of the invention

[0005] In order to improve the problem of poor adhesion of current free radical-curing UV tin printing varnish, the present application provides a high-adhesion free radical-curing UV tin printing varnish and a preparation method thereof.

[0006] In the first aspect, the present application provides a high-adhesion free radical-curing UV iron printing varnish, which adopts the following technical scheme: a high-adhesion free radical-curing UV iron printing varnish, comprising the following components in parts by weight: 45-65 parts of free radical-curing oligomers, 25-44 parts of free radical-curing monomers, 2-4 parts of free radical initiators, 6-10 parts of adhesion promoters, 0.05-0.5 parts of leveling agents, and 0.05-0.5 parts of defoaming agents.

[0007] The present application adopts free radical curing oligomers as the main film-forming substances in UV printing varnish. They can form a polymer network structure through free radical polymerization under ultraviolet light irradiation, giving the varnish excellent mechanical properties, weather resistance and chemical stability; while free radical curing monomers are reactive substances in UV printing varnish. They can quickly undergo polymerization reaction with free radical curing oligomers under ultraviolet light irradiation to further form a cross-linked network structure, thereby enhancing the curing speed and cross-linking density of the varnish. Therefore, the present application adopts a method of cooperating free radical curing oligomers with free radical curing monomers to form a relatively tight network structure during the curing process, thereby reducing the volume shrinkage caused by changes in the distance between molecules, reducing the volume shrinkage rate of UV printing varnish after curing, and significantly improving the adhesion of UV printing varnish to substrates such as white tin and ink.

[0008] Optionally, the free radical curable oligomer is selected from one or more of modified epoxy acrylate resins, polyester acrylates and amino acrylates.

[0009] The modified epoxy acrylate resin has a viscosity of 6500-9000 cps at 25°C, a solid content of ≥98%, and a functionality of 3. The polyester acrylate has a viscosity of 6000-10000 cps at 25°C, a solid content of ≥98%, and a functionality of 2. The amino acrylate has a viscosity of 3000-5000 cps at 25°C, a solid content of ≥98%, and a functionality of 3.

[0010] Optionally, the free radical curing oligomer is selected from one or more of L-6112C of Guangzhou Lankelu New Materials Co., Ltd., SM 6606 of Sanmu, and 6116 of Sanmu.

[0011] Since the modified epoxy acrylate molecular chain contains more rigid groups (such as epoxy and acrylate groups), it can form a relatively tight and rigid network structure after curing. Therefore, the coating formed by the modified epoxy acrylate resin after curing usually has higher hardness and rigidity. Since the polyester acrylate resin contains more flexible segments (such as ester bonds) in its molecular chain, it can maintain good flexibility after curing. In addition, since the base coating white butyl is also a polyester substance, the polyester acrylate and the base coating white butyl have a more rigid structure, and better adhesion can be formed between the two. The amino acrylate molecule contains both amino and acrylate groups, and both groups have strong reactivity. The amino group can form hydrogen bonds or chemical bonds with the surfaces of various substrates, while the acrylate group can cross-link and solidify with other resin molecules in the tinplate varnish through free radical polymerization to form a dense network structure; moreover, during the coating process, amino acrylate can penetrate into the tiny pores on the surface of the substrate to form a mechanical lock. At the same time, the amino groups on its molecular chain form hydrogen bonds or chemical bonds with the polar groups on the surface of the substrate, further enhancing the bonding force between the coating and the substrate.

[0012] Optionally, the free radical curable oligomer comprises modified epoxy acrylate resin, polyester acrylate and amino acrylate in a mass ratio of 5-7:2-4:2.

[0013] The present application uses modified epoxy acrylate resin, polyester acrylate and amino acrylate to mix in the above proportion to obtain a free radical curing oligomer, which can form a free radical curing oligomer system with excellent performance. Among them, the modified epoxy acrylate resin is the leading component, providing the main mechanical performance support; the polyester acrylate is used to improve the hardness and volume shrinkage of the cured film; and the amino acrylate focuses on improving adhesion and promoting the curing reaction.

[0014] Optionally, the free radical curing monomer is selected from one or more of tripropylene glycol diacrylate, pentaerythritol triacrylate and cyclotrimethylolpropane formal acrylate.

[0015] The tripropylene glycol diacrylate molecule contains two acrylate groups connected by a tripropylene glycol chain segment. This structure makes it highly reactive in free radical polymerization reactions. Therefore, the addition of tripropylene glycol diacrylate can increase the curing speed. At the same time, due to its long molecular chain, it helps to increase the flexibility and impact resistance of the cured film. The pentaerythritol triacrylate molecule contains three acrylate groups connected by a multifunctional center of pentaerythritol. This structure enables PETA to form a highly cross-linked network structure in free radical polymerization reactions. Therefore, the addition of pentaerythritol triacrylate can significantly improve the hardness, wear resistance and chemical resistance of the cured film. Cyclotrimethylolpropane formal acrylic acid is a cyclic monomer containing multiple acrylate groups. The formal ring in its structure increases the rigidity and stability of the molecule. Therefore, the addition of cyclotrimethylolpropane formal acrylic acid can improve the hardness and heat resistance of the cured film to a certain extent. At the same time, due to its cyclic structure, it may also have a positive effect on the flexibility and weather resistance of the cured film.

[0016] Optionally, the free radical curing monomer is selected from one or more of Youyang Technology AM-321, Youyang Technology AM-324, Youyang Technology AM-313, and Youyang Technology AM-322.

[0017] Optionally, the free radical curing monomers include tripropylene glycol diacrylate, pentaerythritol triacrylate and cyclotrimethylolpropane formal acrylate in a mass ratio of 15-25:3-5:5-15.

[0018] The present application uses tripropylene glycol diacrylate, pentaerythritol triacrylate and cyclotrimethylolpropane formal acrylate to obtain a free radical curing monomer in the above-mentioned proportion, aiming to balance the various properties of the cured product. Tripropylene glycol diacrylate as the main monomer provides fast curing and good flexibility; the appropriate amount of pentaerythritol triacrylate can improve the hardness and wear resistance; cyclotrimethylolpropane formal acrylate further improves the hardness, heat resistance and weather resistance.

[0019] Optionally, the initiator is selected from one or both of 2-hydroxy-2-methyl-1-phenyl-1-propanone and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.

[0020] Initiators are key components for initiating polymerization reactions. They can absorb light energy (such as ultraviolet light) or heat energy to generate free radicals, which in turn initiate polymerization reactions between monomers and oligomers. 2-Hydroxy-2-methyl-1-phenyl-1-propanone has a high light absorption efficiency and a fast initiation rate. It can quickly decompose under ultraviolet light to generate free radicals, thereby initiating polymerization reactions. 2,4,6-Trimethylbenzoylphenylphosphonic acid ethyl ester has a wide light absorption range and high photoinitiation efficiency. It can absorb ultraviolet light in a wide wavelength range and generate enough free radicals to initiate polymerization reactions.

[0021] Optionally, the initiator comprises 2-hydroxy-2-methyl-1-phenyl-1-propanone and ethyl 2,4,6-trimethylbenzoylphenylphosphonate in a mass ratio of 1-3:1-3.

[0022] The present application adopts the above two initiators in combination, and their ratio can be adjusted according to specific needs to prepare a cured product with excellent performance.

[0023] Optionally, the free radical initiator is one or more of IGM Irgacure 1173 and IGM Irgacure TPO-L.

[0024] Optionally, the adhesion promoter is a chlorinated polyester resin.

[0025] Chlorinated polyester resin has excellent chemical resistance, heat resistance and weather resistance. Chlorination modification makes the resin molecules contain chlorine atoms, which can react chemically with functional groups such as hydroxyl and carboxyl groups on the surface of the substrate to form strong chemical bonds, thereby improving adhesion. In addition, the viscosity of chlorinated polyester resin is 1800cps at 60°C, and its strong polar chlorine functional groups have a strong effect on improving the adhesion of the primer through dispersion.

[0026] Optionally, the adhesion promoter is allnex EBECRYL 41.

[0027] In a second aspect, the present application also provides a method for preparing the high-adhesion free radical-curing UV iron printing varnish, which adopts the following technical solution: A method for preparing the high-adhesion free radical-curing UV iron printing varnish comprises the following steps: Step S1: mixing the free radical curing oligomer, the free radical curing monomer and the adhesion promoter and stirring them uniformly; Step S2: adding the free radical initiator to the mixture obtained in step S1 and stirring; Step S3: adding the leveling agent and the defoaming agent to the mixture obtained in step S2, stirring, and obtaining the mixture.

[0028] Optionally, in step S1, the stirring speed is 1000-1500 rpm, and the stirring time is 30-60 min.

[0029] The preparation method of UV tin printing varnish of the present application has simple steps, convenient operation and easy control. By accurately controlling the order of addition and stirring conditions of each component, the uniform mixing and full reaction of each component of the varnish can be ensured. The method not only improves the production efficiency and quality stability of the varnish, but also reduces production costs and energy consumption. In addition, the method is also suitable for large-scale industrial production, providing an efficient, environmentally friendly and high-quality varnish preparation solution for the tin printing industry.

[0030] In summary, the present application includes at least one of the following beneficial effects: 1. This application maintains the original high efficiency and environmental protection advantages of free radical curing UV iron printing varnish, and ensures that the varnish has excellent film-forming properties and physical properties while rapidly curing by selecting suitable free radical curing oligomers and free radical curing monomers. At the same time, the synergistic effect of these components effectively reduces the volume shrinkage during the curing process. The reduction in volume shrinkage not only reduces the stress between the cured film and the substrate (such as white tin, ink layer), but also avoids problems such as cracks and peeling caused by stress concentration, thereby significantly improving the adhesion between the cured film and the substrate and the overall processing adaptability.

[0031] 2. This application effectively solves the problem of poor adhesion caused by the high volume shrinkage of free radical-cured UV iron printing varnish by introducing a specific proportion of adhesion promoter. The adhesion promoter can enhance the interfacial bonding between the varnish and substrates such as white tin and ink, forming stronger chemical bonds or physical entanglements, thereby significantly improving adhesion. The improved varnish can fit more closely to the surface of the substrate during the curing process, and can maintain stable adhesion performance even in complex or demanding production and processing environments, meeting or exceeding the standard requirements of production and processing.

[0032] 3. The high-adhesion free radical curing UV tin printing varnish system provided by the present application does not contain volatile solvents, has low odor, is environmentally friendly, and has high adhesion to white tin and ink. In addition, the preparation method provided is simple and easy to implement, low in cost, and has high practical application value. DETAILED DESCRIPTION

[0033] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0034] Example 1: Example 1 provides a high-adhesion free radical-curing UV iron printing varnish, and its raw material component formula is shown in Table 1. The preparation method is as follows: A method for preparing the high-adhesion free radical-curing UV iron printing varnish comprises the following steps: Step S1: mixing and stirring the free radical curing oligomer, the free radical curing monomer and the adhesion promoter uniformly at a stirring speed of 1500 rpm for 30 min; Step S2: adding a free radical initiator to the mixture obtained in step S1 and stirring, maintaining the original stirring speed for 30 minutes; Step S3: adding a leveling agent and a defoaming agent to the mixture obtained in step S2, and stirring for 30 minutes to obtain the product.

[0035] Example 2-4: Example 2-4 is basically the same as Example 1, the only difference is the different amounts of raw materials, see Table 1 for details.

[0036] Comparative Examples 1-3: Comparative Examples 1-3 are substantially the same as Example 1, except that the amounts of the raw materials are different. For details, see Table 1.

[0037] Table 1 Amounts of raw material components used in Examples 1-4 and Comparative Examples 1-3 (parts by mass) Performance test: The UV tinplate varnish prepared in Examples 1-4 and Comparative Examples 1-3 were respectively roller-coated on the tinplate coated with the primer (ink & white tin) with a thickness of 6 microns. The UV tinplate varnish prepared in Examples and Comparative Examples was heated at 200 mJ / m 2 The energy was used for light curing in a crawler-type mercury lamp curing machine. The performance was measured after curing. The properties of the coating are shown in Table 2.

[0038] 1. Pencil hardness: Pencil hardness is tested according to GB / T6739-2006 and the paint film pencil method is used to evaluate the hardness of the coating.

[0039] 2. Adhesion grade: The adhesion grade is based on the cross-cut test of the paint film in accordance with GB / T 9286-2021 to evaluate the adhesion of the coating.

[0040] 3. Anti-scratch test: The anti-scratch test is carried out according to GB / T9279-2007 and is tested using a QGZ paint film scratch tester to evaluate the anti-scratch performance of the coating.

[0041] 4. Impact test: refer to the standard ASTM D2794-93 for impact test to evaluate the mechanical strength of the coating. During the test, the impact steel ball (20mm diameter, 1kg x 2) is raised to a height of 50cm, and the hammer is allowed to fall freely from the specified height. The punch hits the sample to form a pit. The coating on the protruding part is checked visually or with a specified magnifying glass to see if there is any cracking, which is used to evaluate the impact resistance of the coating.

[0042] 5. T-bending test: The T-bending test is carried out according to GB / T30791-2014 and is used to evaluate the flexibility of the coating.

[0043] Table 2 Performance test results of Examples 1-4 and Comparative Examples 1-3 Test items Experimental Example 1 Experimental Example 2 Experimental Example 3 Experimental Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Pencil hardness 2H 2H 2H 2H 2H 3H 2H Adhesion grade 0 0 0 0 2 2 1 Scratch resistance test 1600g 1600g 1600g 1600g 1600 1700g 1500g Impact test No cracking No cracking No cracking No cracking No cracking Cracking No cracking T-bend 0T 0T 0T 0T 1T 1T 1T It can be seen from the results in Table 2 that the UV iron printing varnish coatings prepared in Examples 1-4 of the present application performed well in tests such as pencil hardness, adhesion, scratch resistance, impact test and T-bend, and have excellent physical properties and stability.

[0044] Compared with Example 1, since the phosphate-modified acrylic resin is used as the adhesion promoter in Comparative Example 1, its adhesion is greatly reduced, and the result of the T-bending test is 1T, indicating that in the free radical curing system provided in the present application, the adhesion promoting effect of the phosphate-modified acrylic resin is poor, and it also indirectly indicates that the adhesion promoting effect of the chlorinated polyester resin is better, which is mainly derived from the strong polar chlorine group and double bond contained in the chlorinated polyester resin (Zhanxin EBECRYL 418). The chlorine group is a strong polar group and can form a strong physical bond with the primer white cotin. The double bond can form a cross-linked network with other double bond-containing monomers in the coating, thereby greatly enhancing the adhesion of the coating.

[0045] Compared with Example 1, Comparative Example 2 improves its pencil hardness and scratch resistance due to the replacement of polyester acrylate with an equal amount of modified epoxy acrylate resin, but its adhesion, impact resistance and flexibility are poor. The main reason is that there are more rigid groups and fewer flexible groups in the free radical curing system, so the coating shows higher rigidity but lacks flexibility, so the coating will crack in the impact test, and the adhesion level is also low. It also indirectly shows that the ratio of the free radical curing oligomer provided in the examples of the present application is relatively reasonable, balancing the ratio of flexible groups to rigid groups in the system, so that the coating has both good adhesion, flexibility, pencil hardness and scratch resistance.

[0046] Compared with Example 1, since the cyclotrimethylolpropane formal acrylate is replaced by an equal amount of tripropylene glycol diacrylate in Comparative Example 3, its adhesion is reduced, the scratch resistance is reduced, and the result of the T-bending test is 1T, indicating that the overall performance of the coating prepared with cyclotrimethylolpropane formal acrylate as the free radical curing monomer is better. The reason may be that cyclotrimethylolpropane formal acrylate has a chemical structure closer to the modified epoxy acrylate resin in the free radical curing system, so it has better compatibility with the system, and the curing reaction is more complete, thus showing better adhesion and mechanical properties.

[0047] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A high-adhesion free radical-curing UV iron printing varnish, characterized in that: The invention comprises the following components in parts by weight: 45-65 parts of free radical curing oligomer, 25-44 parts of free radical curing monomer, 2-4 parts of free radical initiator, 6-10 parts of adhesion promoter, 0.05-0.5 parts of leveling agent and 0.05-0.5 parts of defoaming agent.

2. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The free radical curing oligomer is selected from one or more of modified epoxy acrylate resin, polyester acrylate and amino acrylate.

3. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The free radical curing oligomer comprises modified epoxy acrylate resin, polyester acrylate and amino acrylate in a mass ratio of 5-7:2-4:

2.

4. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The free radical curing monomer is selected from one or more of tripropylene glycol diacrylate, pentaerythritol triacrylate and cyclotrimethylolpropane formal acrylate.

5. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The free radical curing monomers include tripropylene glycol diacrylate, pentaerythritol triacrylate and cyclotrimethylolpropane formal acrylate in a mass ratio of 15-25:3-5:5-15.

6. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The initiator is selected from one or both of 2-hydroxy-2-methyl-1-phenyl-1-propanone and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.

7. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The initiator comprises 2-hydroxy-2-methyl-1-phenyl-1-propanone and ethyl 2,4,6-trimethylbenzoylphenylphosphonate in a mass ratio of 1-3:1-3.

8. The high-adhesion free radical curing UV iron printing varnish according to claim 1, characterized in that: The adhesion promoter is a chlorinated polyester resin.

9. A method for preparing a high-adhesion free radical-curing UV iron printing varnish as claimed in any one of claims 1 to 8, comprising the following steps: Step S1: mixing the free radical curing oligomer, the free radical curing monomer and the adhesion promoter and stirring them uniformly; Step S2: adding the free radical initiator to the mixture obtained in step S1 and stirring; Step S3: adding the leveling agent and the defoaming agent to the mixture obtained in step S2, stirring, and obtaining the mixture.

10. The method for preparing the high-adhesion free radical-curing UV iron printing varnish according to claim 9, wherein in step S1, the stirring speed is 1000-1500 rpm and the stirring time is 30-60 min.

Citation Information

Patent Citations

  • Method for producing ultraviolet curing coating

    CN101418149A

  • Photocuring composition for metal surface and composition containing photocuring composition

    CN110317483A

  • Ultraviolet photocureable coating for polyurethane glass fiber composite material

    CN116333570A