Polyurethane single-component adhesive for co-extrusion plate lamination and preparation method of polyurethane single-component adhesive

By using polyurethane single-component adhesive with high initial adhesive TPU, chlorine acetic resin and acrylic, the problems of low bonding strength and formaldehyde release in coextruded plate bonding are solved, and efficient and environmentally friendly bonding effect is achieved , suitable for a variety of harsh conditions and chemical environments.

CN119060638APending Publication Date: 2024-12-03CHONGQING HANTUO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235897.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing adhesives have low bonding strength during co-extruded board bonding, which can easily lead to the tilt of the board and release formaldehyde during use, causing environmental pollution.

Method used

A polyurethane single-component adhesive, including high-primary TPU, chlorine-vine resin, acrylic acid and dilution solvent, is prepared by a specific stirring and heating vacuum baking process to form a adhesive with high bond strength and durability. agent.

Benefits of technology

Improve construction efficiency, enhance bonding strength and stability, and maintain performance in harsh environments. It is suitable for bonding of substrates with different thermal expansion coefficients. It has excellent buffering and shock absorption functions, and produces almost no volatile organic matter, reducing The impact on the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060638A_ABST
    Figure CN119060638A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyurethane preparation, and particularly discloses a polyurethane single-component adhesive for co-extrusion plate lamination and a preparation method, the polyurethane single-component adhesive is convenient to use, does not need a complex mixing process, can be directly applied to a base material needing to be bonded, can adapt to bonding of base materials with different thermal expansion coefficients, has very high bonding strength, and can be applied to co-extrusion plate lamination. The adhesive can bear large tensile force and shearing force, is suitable for various structural bonding, ensures the bonding firmness and durability, not only has excellent initial bonding strength and final bonding strength, but also has excellent buffering and damping functions, has good tolerance to chemical substances such as acid, alkali, oil, water and the like, and can be widely applied to the field of adhesive bonding. The adhesive can keep stable performance in various chemical environments, is suitable for fitting of artificial large plates such as co-extrusion plates and skinning plates, solves the problems of difficult bonding and easy end warping, and does not release formaldehyde in the use process, so that the pollution to the environment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane preparation, and in particular to a polyurethane single-component adhesive for co-extruded board lamination and a preparation method thereof. Background Art

[0002] Co-extruded board is a composite board formed by extruding two or more different materials through an extruder. The production process of this board is based on the extrusion principle, that is, two or more molten materials pass through the same extruder nozzle of the extruder at the same time, and then cool and form in the mold. Co-extruded board has many excellent properties, which makes it widely used in many fields such as construction, transportation, electronics, packaging, etc. Adhesives need to be added during the bonding process of co-extruded boards.

[0003] Adhesives refer to a class of natural or synthetic, organic or inorganic substances that can connect two or more parts or materials together through interfacial adhesion and cohesion.

[0004] However, the existing adhesives have low bonding strength, which can easily cause the boards to warp, and release formaldehyde when used, thus causing environmental pollution. Summary of the invention

[0005] The purpose of the present invention is to provide a polyurethane one-component adhesive for co-extruded board bonding and a preparation method, aiming to solve the technical problems in the prior art that the adhesive has low bonding strength, easily causes the board to warp, and releases formaldehyde during use, thereby causing environmental pollution.

[0006] To achieve the above object, the present invention adopts a polyurethane one-component adhesive for co-extruded board bonding, which includes the following components: high initial viscosity TPU, chloroacetic acid resin, acrylic acid and diluent solvent.

[0007] Among them, the portion of the high initial viscosity TPU is 15-25 parts, the portion of the chloroacetic acid resin is 8-15 parts, the portion of the acrylic acid is 2-5 parts, and the portion of the diluent solvent is 60-75 parts.

[0008] Preferably, 15-25 parts of the high initial viscosity TPU and 8-15 parts of the chlorovinyl resin are stirred for reaction, then 2-5 parts of the acrylic acid are added, and finally 60-75 parts of the dilution solvent are added for dilution.

[0009] The high initial viscosity TPU comprises the following components: polyester polyol, chain extender, isocyanate and antioxidant.

[0010] Among them, the polyester polyol accounts for 80-90 parts, the chain extender accounts for 1-1.5 parts, the isocyanate accounts for 10-19 parts, and the antioxidant accounts for 0.5 parts.

[0011] Preferably, 10-19 parts of the isocyanate and 80-90 parts of the polyester polyol are stirred to react to generate a prepolymer, and then 1-1.5 parts of the chain extender and 0.5 parts of the antioxidant are added to the generated prepolymer, and then heated and vacuum dehydrated, poured into a preheated container and rapidly stirred, and then heated and vacuum baked, and finally cooled to obtain the high initial viscosity TPU material.

[0012] The present invention also provides a method for preparing a polyurethane one-component adhesive for co-extruded board lamination, and the preparation of the polyurethane one-component adhesive for co-extruded board lamination as described above comprises the following steps:

[0013] Step 1: Take polyester polyol, chain extender, isocyanate and antioxidant in proportion and set aside;

[0014] Step 2: Put the polyester polyol and isocyanate obtained in step 1 into a reaction kettle and stir and mix;

[0015] Step 3: adding the chain extender obtained in step 1 into the reactor;

[0016] Step 4: adding the antioxidant obtained in step 1 into the reaction kettle;

[0017] Step 5: Then heat the reactor for vacuum dehydration;

[0018] Step 6: Then put the dehydrated polyester polyol, chain extender, isocyanate and antioxidant into a preheated container, stir quickly, and then heat and vacuum bake;

[0019] Step 7: After cooling, the high initial viscosity TPU material is obtained;

[0020] Step 8: Take high initial viscosity TPU, chloroacetic acid resin, acrylic acid and dilution solvent in proportion for later use;

[0021] Step 9: Add the high initial viscosity TPU, chloroacetic acid resin and acrylic acid obtained in step 1 into the reactor to react;

[0022] Step 10: Add the dilution solvent obtained in step 1 to dilute, and then continue to stir and mix to obtain the polyurethane single-component adhesive material.

[0023] Wherein, in step five, the temperature at which the reactor is heated is 100-120°C.

[0024] Wherein, in step six, the temperature at which the container is heated is 130-150°C.

[0025] Wherein, in step seven, the container is cooled to 20-30°C.

[0026] Wherein, in step ten, the stirring time is 1-2 hours.

[0027] The beneficial effects of the present invention are as follows: the present invention is easy to use, does not require a complicated mixing process, can be directly applied to a substrate that needs to be bonded, thereby improving construction efficiency, and is resistant to aging, UV rays, and ozone, and can maintain stable performance under various severe climatic conditions. It can quickly solidify under appropriate conditions to form a stable bonding layer, and can adapt to the bonding of substrates with different thermal expansion coefficients. It has very high bonding strength, can withstand large tensile and shear forces, and is suitable for various structural bondings to ensure the firmness and durability of the bonding. It not only has excellent initial adhesion and final bonding strength, but also has excellent buffering and shock absorbing functions, has good tolerance to chemical substances such as acid, alkali, oil, and water, and can maintain stable performance in various chemical environments. It is suitable for the bonding of large artificial boards such as co-extruded boards and crusted boards, and solves the problems of difficult bonding and easy warping. In addition, almost no volatile organic compounds are generated during the use of the present invention, and the impact on the environment is relatively small. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a step flow chart of Example 1 of the present invention.

[0030] Figure 2 It is a step flow chart of Example 2 of the present invention.

[0031] Figure 3 It is a step flow chart of Example 3 of the present invention. DETAILED DESCRIPTION

[0032] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0033] The invention provides a polyurethane one-component adhesive for co-extruded board lamination and a preparation method thereof. The polyurethane one-component adhesive for co-extruded board lamination is composed of the following raw materials: high initial viscosity TPU, chloroacetic acid resin, acrylic acid and a diluent solvent.

[0034] The proportion of the high initial viscosity TPU is 15-25 parts, the proportion of the chloroacetic acid resin is 8-15 parts, the proportion of the acrylic acid is 2-5 parts, and the proportion of the diluent solvent is 60-75 parts.

[0035] The high initial viscosity TPU is composed of the following raw materials: polyester polyol, chain extender, isocyanate and antioxidant.

[0036] The polyester polyol accounts for 80-90 parts, the chain extender accounts for 1-1.5 parts, the isocyanate accounts for 10-19 parts, and the antioxidant accounts for 0.5 parts.

[0037] Embodiment 1:

[0038] See also Figure 1 , Figure 1 is a flow chart of the steps of Example 1 of the present invention. The present invention also provides a method for preparing a polyurethane one-component adhesive for co-extruded board bonding, preparing the polyurethane one-component adhesive for co-extruded board bonding as described above,

[0039] The steps include:

[0040] Step 1: Take 80 parts of polyester polyol, 1 part of chain extender, 10 parts of isocyanate and 0.5 parts of antioxidant in proportion for later use;

[0041] Step 2: Put 80 parts of polyester polyol and 10 parts of isocyanate taken in step 1 into a reaction kettle and stir for 0.5 hours;

[0042] Step 3: Add 1 portion of the chain extender taken in step 1 into the reactor;

[0043] Step 4: Add 0.5 parts of the antioxidant taken in step 1 into the reactor;

[0044] Step 5: Then heat the reactor to 100°C for vacuum dehydration;

[0045] Step 6: Then put the dehydrated polyester polyol, chain extender, isocyanate and antioxidant into a preheated container and stir rapidly for 15 minutes, then heat the container to 130° C. for vacuum baking;

[0046] Step 7: Wait until the container is cooled to 20° C. to obtain the high initial viscosity TPU material;

[0047] Step 8: Take 15 parts of high initial viscosity TPU, 8 parts of chloroacetic acid resin, 2 parts of acrylic acid and 60 parts of dilution solvent according to the proportion for use;

[0048] Step 9: Add 15 parts of high initial viscosity TPU, 8 parts of chloroacetic acid resin and 2 parts of acrylic acid taken in step 1 into the reactor to react;

[0049] Step 10: Add 60 parts of the dilution solvent taken in step 1 for dilution, and then continue stirring for 1 hour to obtain the polyurethane one-component adhesive material.

[0050] The present invention provides a polyurethane one-component adhesive for co-extruded board bonding and a preparation method. The present invention is easy to use, does not require a complicated mixing process, can be directly applied to a substrate to be bonded, improves construction efficiency, is resistant to aging, UV rays, and ozone, can maintain stable performance under various severe climatic conditions, can quickly solidify under appropriate conditions to form a stable bonding layer, can adapt to the bonding of substrates with different thermal expansion coefficients, has very high bonding strength, can withstand large tensile and shear forces, is suitable for various structural bonding, ensures the firmness and durability of the bonding, not only has excellent initial adhesion and final bonding strength, but also has excellent buffering and shock absorbing functions, has good tolerance to chemical substances such as acid, alkali, oil, water, etc., can maintain stable performance in various chemical environments, is suitable for the bonding of co-extruded boards, crusted boards and other artificial large boards, solves the problems of difficult bonding and easy warping, and almost no volatile organic compounds are generated during the use of the present invention, and the impact on the environment is relatively small.

[0051] Embodiment 2:

[0052] See also Figure 2 , Figure 2 is a flow chart of the steps of Example 2 of the present invention. The present invention also provides a method for preparing a polyurethane one-component adhesive for co-extruded board bonding, preparing the polyurethane one-component adhesive for co-extruded board bonding as described above,

[0053] The steps include:

[0054] Step 1: Take 90 parts of polyester polyol, 1.5 parts of chain extender, 19 parts of isocyanate and 0.5 parts of antioxidant in proportion for later use;

[0055] Step 2: Put 90 parts of polyester polyol and 19 parts of isocyanate taken in step 1 into a reaction kettle and stir for 0.5 hours;

[0056] Step 3: Add 1.5 parts of the chain extender taken in step 1 into the reactor;

[0057] Step 4: Add 0.5 parts of the antioxidant taken in step 1 into the reactor;

[0058] Step 5: Then heat the reactor to 120°C for vacuum dehydration;

[0059] Step 6: Then put the dehydrated polyester polyol, chain extender, isocyanate and antioxidant into a preheated container and stir rapidly for 15 minutes, then heat the container to 150° C. for vacuum baking;

[0060] Step 7: Waiting for the container to cool to 30° C. to obtain the high initial viscosity TPU material;

[0061] Step 8: Take 25 parts of high initial viscosity TPU, 15 parts of chloroacetic acid resin, 5 parts of acrylic acid and 75 parts of dilution solvent in proportion for use;

[0062] Step 9: Add 25 parts of high initial viscosity TPU, 15 parts of chloroacetic acid resin and 5 parts of acrylic acid taken in step 1 into the reactor to react;

[0063] Step 10: Add 75 parts of the dilution solvent taken in step 1 for dilution, and then continue stirring for 2 hours to obtain the polyurethane one-component adhesive material.

[0064] The present invention provides a polyurethane one-component adhesive for co-extruded board bonding and a preparation method. The present invention is easy to use, does not require a complicated mixing process, can be directly applied to a substrate to be bonded, improves construction efficiency, is resistant to aging, UV rays, and ozone, can maintain stable performance under various severe climatic conditions, can quickly solidify under appropriate conditions to form a stable bonding layer, can adapt to the bonding of substrates with different thermal expansion coefficients, has very high bonding strength, can withstand large tensile and shear forces, is suitable for various structural bonding, ensures the firmness and durability of the bonding, not only has excellent initial adhesion and final bonding strength, but also has excellent buffering and shock absorbing functions, has good tolerance to chemical substances such as acid, alkali, oil, water, etc., can maintain stable performance in various chemical environments, is suitable for the bonding of co-extruded boards, crusted boards and other artificial large boards, solves the problems of difficult bonding and easy warping, and almost no volatile organic compounds are generated during the use of the present invention, and the impact on the environment is relatively small.

[0065] Embodiment 3:

[0066] See also Figure 3 , Figure 3 is a flow chart of the steps of Example 3 of the present invention. The present invention also provides a method for preparing a polyurethane one-component adhesive for co-extruded board bonding, preparing the polyurethane one-component adhesive for co-extruded board bonding as described above,

[0067] The steps include:

[0068] Step 1: Take 85 parts of polyester polyol, 1.25 parts of chain extender, 14.5 parts of isocyanate and 0.5 parts of antioxidant in proportion for later use;

[0069] Step 2: Put 85 parts of polyester polyol and 14.5 parts of isocyanate taken in step 1 into a reaction kettle and stir for 0.5 hour;

[0070] Step 3: Add 1.25 parts of the chain extender taken in step 1 into the reactor;

[0071] Step 4: Add 0.5 parts of the antioxidant taken in step 1 into the reactor;

[0072] Step 5: Then heat the reactor to 110°C for vacuum dehydration;

[0073] Step 6: Then put the dehydrated polyester polyol, chain extender, isocyanate and antioxidant into a preheated container and stir rapidly for 15 minutes, then heat the container to 140° C. for vacuum baking;

[0074] Step 7: Wait until the container is cooled to 25° C. to obtain the high initial viscosity TPU material;

[0075] Step 8: Take 20 parts of high initial viscosity TPU, 11.5 parts of chloroacetic acid resin, 3.5 parts of acrylic acid and 67.5 parts of dilution solvent in proportion for use;

[0076] Step 9: Add 20 parts of high initial viscosity TPU, 11.5 parts of chloroacetic acid resin and 3.5 parts of acrylic acid taken in step 1 into the reactor to react;

[0077] Step 10: Add 67.5 parts of the dilution solvent taken in step 1 for dilution, and then continue stirring for 1.5 hours to obtain the polyurethane one-component adhesive material.

[0078] The present invention provides a polyurethane one-component adhesive for co-extruded board bonding and a preparation method. The present invention is easy to use, does not require a complicated mixing process, can be directly applied to a substrate to be bonded, improves construction efficiency, is resistant to aging, UV rays, and ozone, can maintain stable performance under various severe climatic conditions, can quickly solidify under appropriate conditions to form a stable bonding layer, can adapt to the bonding of substrates with different thermal expansion coefficients, has very high bonding strength, can withstand large tensile and shear forces, is suitable for various structural bonding, ensures the firmness and durability of the bonding, not only has excellent initial adhesion and final bonding strength, but also has excellent buffering and shock absorbing functions, has good tolerance to chemical substances such as acid, alkali, oil, water, etc., can maintain stable performance in various chemical environments, is suitable for the bonding of co-extruded boards, crusted boards and other artificial large boards, solves the problems of difficult bonding and easy warping, and almost no volatile organic compounds are generated during the use of the present invention, and the impact on the environment is relatively small.

[0079] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A polyurethane one-component adhesive for co-extruded board lamination, characterized in that: The composition includes: high initial viscosity TPU, chloroacetic acid resin, acrylic acid and diluent.

2. The polyurethane one-component adhesive for co-extruded board lamination according to claim 1, The proportion of the high initial viscosity TPU is 15-25 parts, the proportion of the chloroacetic acid resin is 8-15 parts, the proportion of the acrylic acid is 2-5 parts, and the proportion of the diluent solvent is 60-75 parts.

3. The polyurethane one-component adhesive for co-extruded board lamination according to claim 2, characterized in that: The high initial viscosity TPU comprises the following components: polyester polyol, chain extender, isocyanate and antioxidant.

4. The polyurethane one-component adhesive for co-extruded board lamination according to claim 3, characterized in that: The polyester polyol accounts for 80-90 parts, the chain extender accounts for 1-1.5 parts, the isocyanate accounts for 10-19 parts, and the antioxidant accounts for 0.5 parts.

5. A method for preparing a polyurethane one-component adhesive for co-extruded board lamination, comprising preparing the polyurethane one-component adhesive for co-extruded board lamination as claimed in claim 4, characterized in that: The steps include: Step 1: Take polyester polyol, chain extender, isocyanate and antioxidant in proportion and set aside; Step 2: Put the polyester polyol and isocyanate obtained in step 1 into a reaction kettle and stir and mix; Step 3: adding the chain extender obtained in step 1 into the reactor; Step 4: adding the antioxidant obtained in step 1 into the reaction kettle; Step 5: Then heat the reactor for vacuum dehydration; Step 6: Then put the dehydrated polyester polyol, chain extender, isocyanate and antioxidant into a preheated container, stir quickly, and then heat and vacuum bake; Step 7: After cooling, the high initial viscosity TPU material is obtained; Step 8: Take high initial viscosity TPU, chloroacetic acid resin, acrylic acid and dilution solvent in proportion for later use; Step 9: Add the high initial viscosity TPU, chloroacetic acid resin and acrylic acid obtained in step 1 into the reactor to react; Step 10: Add the dilution solvent obtained in step 1 to dilute, and then continue to stir and mix to obtain the polyurethane single-component adhesive material.

6. The method for preparing the polyurethane one-component adhesive for co-extruded board lamination according to claim 5, characterized in that: In step five, the temperature of heating the reactor is 100-120°C.

7. The polyurethane one-component adhesive for co-extruded board lamination and the preparation method thereof according to claim 6, characterized in that: In step six, the temperature at which the container is heated is 130-150°C.

8. The method for preparing the polyurethane one-component adhesive for co-extruded board lamination according to claim 7, characterized in that: In step seven, the container is cooled to 20-30°C.

9. The method for preparing the polyurethane one-component adhesive for co-extruded board lamination according to claim 8, characterized in that: In step ten, the stirring time is 1-2 hours.