Single-component epoxy-thiol system adhesive and preparation method thereof
By using hyperbranched polymers with anhydride groups in epoxy resin adhesives in synergistically with core-shell resins, the brittleness and storage stability of epoxy resins are solved, and a high modulus, high toughness and high reactivity adhesive is achieved. Suitable for the applications of the new generation of electronic consumer devices.
Patent Information
- Application Number
- CN202310649094.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
The brittleness of epoxy resin limits its application in high-tech fields. Traditional toughening methods cannot meet the high modulus, high toughness, high reactivity and stability requirements of adhesives at the same time, and it is difficult to prepare hyperbranched polymers into a single component. Epoxy-thiol system adhesives have storage stability problems.
Hyperbranched polymer with end groups with acid anhydride groups as synergistically interacts with core-shell resin to obtain hyperbranched polymer through Grubbs catalyst reaction, and core-shell resin, curing agent and accelerator are added to the adhesive formulation to form a single component ring Oxygen-thiol system adhesive improves shear strength and toughness while maintaining storage stability.
The stability and drop resistance under high and low temperature conditions have been achieved, which significantly improves the shear strength and toughness of the adhesive, while avoiding storage stability issues.
Smart Images

Figure CN119060664A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of adhesives, and in particular to a one-component epoxy-thiol system adhesive and a preparation method thereof. Background Art
[0002] Epoxy resin is a highly versatile and unique polymer material, which is favored by the industry for its excellent adhesion, outstanding corrosion resistance and excellent dielectric insulation. It is widely used in the manufacturing of various products such as coatings, composite materials, casting materials, adhesives, molding materials and injection molding materials.
[0003] However, the brittle nature of epoxy resins has largely limited their application in many high-tech fields. Therefore, toughening and modifying epoxy resins to improve their brittleness has become a key challenge that needs to be urgently addressed in the industry. The toughening methods that can be used include: toughening with traditional rubber and core-shell rubber, toughening with thermoplastic resins, toughening with hyperbranched resins, toughening with interpenetrating networks, and toughening with nanofillers.
[0004] Considering the application scenarios of the new generation of electronic consumer devices, the adhesives required are required to have: high modulus, high toughness, high reactivity, and stability of the cross-linked products under high and low temperature (frequency) conditions. High modulus means a higher cross-linking density in the network; high toughness means longer molecular chains between cross-linking points; high reactivity means abundant reactive sites with high activity. However, for traditional small molecule adhesives and linear polymer adhesives, due to their molecular size and topological structure, they cannot meet the requirements of modulus, toughness, reactivity, and stability at the same time. Other fillers need to be added to the adhesive system to meet actual needs. This will cause new problems of incompatibility between the adhesive system and other fillers, which will affect the properties of the acoustic material.
[0005] The viscosity of the core-shell resin material itself is relatively high, and the wettability to the surface of the bonding substrate is poor, which affects the shear strength performance of the adhesive. The synthesis process of hyperbranched polymers is relatively complicated, resulting in high production costs; in addition, if the hyperbranched chain segments are not long enough, the impact force cannot be effectively buffered and dispersed, so that the toughness performance is poor. In CN113943473A, hyperbranched polyamide esters, core-shell resins and island-type toughening agents are used to greatly improve the toughness of the material and the mechanical properties are also improved to a certain extent, but the hyperbranched polymers selected cannot be prepared into a single-component epoxy-thiol system adhesive due to the reactivity of their functional groups; because it has the problem of poor storage stability. Summary of the invention
[0006] The object of the present invention is to provide a one-component epoxy-thiol system adhesive and a preparation method thereof.
[0007] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0008] In one aspect, the present invention provides a one-component epoxy-thiol system adhesive, which comprises the following raw materials in parts by weight:
[0009]
[0010] The hyperbranched polymer is a polyolefin having anhydride groups as terminal groups.
[0011] According to some specific embodiments of the present invention, the anhydride group is preferably succinic anhydride
[0012] According to some specific embodiments of the present invention, the hyperbranched polymer is obtained by reacting 3-allyl-cyclooctene and itaconic anhydride in the presence of a Grubbs catalyst.
[0013] The present invention adds core-shell resin and a specific type of hyperbranched polymer to the adhesive formula, which can exert a synergistic effect between them. The hyperbranched polymer increases the cross-linking sites on the surface of the substrate, and the core-shell particles effectively disperse and transmit the impact force, thereby simultaneously improving the shear strength, the strength of the colloid itself and the toughness performance.
[0014] According to some specific embodiments of the present invention, the adhesive comprises the following raw materials in parts by weight:
[0015]
[0016] According to some specific embodiments of the present invention, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, novolac epoxy resin and alicyclic epoxy resin.
[0017] According to some specific embodiments of the present invention, the core of the core-shell resin is selected from butadiene (BD), butyl acrylate (BA), Si (silicon), styrene (ST) or rubber (such as polybutadiene rubber), and the shell is selected from acrylics, styrene (ST), acrylonitrile (AN), reactive monomers, etc. For example, at least one of MX-125, MX-154, MX-254, MX-257 of Kaneka Company of Japan, W35 of Wacker Company of Germany, or EXL-2314, EXL-2655 of DOW Company of the United States can be selected.
[0018] According to some specific embodiments of the present invention, the curing agent is a thiol curing agent, selected from at least one of trimethylolpropane tris(3-mercaptopropionate), 1,4-butanediol di(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), ethylene glycol di(3-mercaptopropionate), trithiol mercaptan, tetrafunctional secondary mercaptan PE1, and polythiol. For example, at least one of Karenz MT PE1 of Showa Corporation of Japan and Thiocure 330, 331, 332, 340, 341, and 360 of Bruno Bock of Germany can be selected.
[0019] According to some specific embodiments of the present invention, the accelerator is a latent accelerator, preferably at least one of FXR-1020, FXR-1030, FXR-1081 (produced by Fuji Chemical Co., Ltd. of Japan), PN-23, PN-40, MY-24 (produced by Ajinomoto Fine Chemicals Co., Ltd. of Japan), EH-4337S, EH-4360S (produced by ADK of Japan).
[0020] According to some specific embodiments of the present invention, the stabilizer is preferably at least one selected from ICAM-8401, ICAM-8402 (produced by Shenzhen Chuchuang Applied Materials Co., Ltd.), HSCHEM-3200 (produced by Hesheng Chemical), and NP-100 (produced by Japan SANAPRO).
[0021] According to some specific embodiments of the present invention, the adhesive comprises the following raw materials in parts by weight:
[0022]
[0023] Another aspect of the present invention provides a method for preparing one or more one-component epoxy-thiol system adhesives, comprising the following steps:
[0024] The epoxy resin, the hyperbranched polymer, the core-shell resin, the stabilizer, the curing agent and the accelerator are uniformly mixed to obtain the one-component epoxy-thiol system adhesive.
[0025] According to some specific embodiments of the present invention, the preparation method specifically includes the following process:
[0026] The epoxy resin, the hyperbranched polymer and the core-shell resin are added into the reactor, and stirred for 1 to 2 hours to mix evenly; after cooling the materials to below 30° C., a stabilizer is added and stirring is continued for 10 to 30 minutes; the materials are cooled to below 30° C. again, and then a curing agent and an accelerator are added, and stirred for 1 to 2 hours to mix evenly, so as to obtain the one-component epoxy-thiol system adhesive.
[0027] According to some specific embodiments of the present invention, the preparation method further comprises: packaging the obtained one-component epoxy-thiol system adhesive into a rubber cartridge and sealing it to obtain a finished product, and the finished product is stored at a low temperature below -20°C.
[0028] In the adhesive provided by the present invention, the core-shell resin and the specific type of hyperbranched polymer have a synergistic effect, the hyperbranching is used to increase the cross-linking sites with the substrate surface, and the core-shell resin is used to effectively disperse and transmit the impact force to a large extent, while improving the shear strength, adhesive body strength and toughness performance. The hyperbranched polymer of the present invention can be applied to a single-component epoxy-thiol system without causing it to have storage stability problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the H-NMR spectrum of the hyperbranched polymer TM27-d.
[0030] Figure 2 Infrared spectrum of hyperbranched polymer TM27-d. DETAILED DESCRIPTION
[0031] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0032] All numerical specifications herein (e.g., temperature, time, concentration, and weight, etc., including ranges for each thereof) are generally approximate values that may be appropriately varied (+) or (-) in increments of 0.1 or 1.0. All numerical specifications may be understood as being preceded by the term "about."
[0033] The raw materials used in the following examples and comparative examples are as follows:
[0034] Epoxy resin: Nan Ya Plastics NPEL-128;
[0035] Core-shell resin: MX-154 from Kaneka, Japan;
[0036] Thiol: Thiocure 330 from Bruno Bock, Germany;
[0037] Latent accelerator: FXR-1081 from Fuji Corporation of Japan;
[0038] Stabilizer: HSCHEM-3200 from Hesheng Chemical;
[0039] Hyperbranched polymer NJ292: purchased from Weihai Chenyuan Molecular New Materials Co., Ltd.
[0040] Hyperbranched polymer TM27-d is a polyolefin with succinic anhydride as the terminal functional group, and its schematic structural formula is as follows:
[0041]
[0042] The specific values of m and n vary according to different synthesis conditions, n is 5 to 600, and m is 1 to 2. The repeating unit represented by m refers to the part above the bracket, including n.
[0043] Hyperbranched polymer TM27-d was prepared by the following steps:
[0044] 3-allyl-cyclooctene (1 mmol in 1 mL tetrahydrofuran) was placed in a 2 mL sample bottle, Grubbs second generation catalyst (4.43 mg, dissolved in 20 μL tetrahydrofuran) and itaconic anhydride (17.41 mg, dissolved in 100 μL tetrahydrofuran) were added, and the reaction was carried out under argon for 24 h (reaction temperature was 50° C.), and then 0.5 mL of vinyl ethyl ether / tetrahydrofuran solution (v:v=50%) was added to terminate the reaction to obtain a hyperbranched polymer TM27-d, in which n was 26, m was 1, and the monomer conversion rate was 64.3%. Figure 1 The branching degree of the product was 18.2% as characterized by H-NMR. Figure 2 Infrared spectroscopy confirmed that the polymer contained anhydride groups.
[0045] Hyperbranched polymer H2M, compared with hyperbranched polymer TM27-d, has a hydroxyl terminal group, and the raw material itaconic anhydride is replaced with cis-2-butene-1,4-diol, and is prepared by the following steps:
[0046] Take 3-allyl-cyclooctene (1 mmol in 1 mL of tetrahydrofuran), place it in a 2 mL sample bottle, add Grubbs second-generation catalyst (3.13 mg, dissolved in 20 μL of tetrahydrofuran) and cis-2-butene-1,4-diol (4.41 mg, dissolved in 20 μL of tetrahydrofuran), react under argon for 24 h (reaction temperature is 50°C), and then add 0.5 mL of vinyl ethyl ether / tetrahydrofuran solution (v:v=50%) to terminate the reaction to obtain a hyperbranched polymer H2M.
[0047] The performance tests involved in the following embodiments and comparative examples include:
[0048] Viscosity change rate: After the adhesive is prepared, the viscosity is first measured using a Brookfield RVT with a #52 rotor at 25°C. The viscosity at this time is taken as the initial viscosity. The adhesive is then placed at room temperature for 7 consecutive days and then the viscosity is measured using the same method. The viscosity after 7 days is compared with the initial viscosity to obtain the viscosity change rate.
[0049] The zinc-nickel shear strength test method is in accordance with the national standard GB7124-86.
[0050] Drop test method: Apply adhesive between two electronic components and then cure them. Place the cured product workpiece on a directional drop tester. According to GB / T2423.8 standard, the test conditions are: directional drop height of 1.67 meters, the falling ground material is iron, and a drop test is performed. Finally, the number of drops when the product fails is recorded.
[0051] Note: When conducting parallel comparison experiments, it is necessary to ensure that the weight / shape of each tested product remains consistent. Otherwise, the impact force on different products will be inconsistent, and the experimental results will also be different.
[0052] Examples and Comparative Examples
[0053] A one-component epoxy-thiol system adhesive comprises the following processes:
[0054] Add epoxy resin NPEL-128, core-shell resin MX-154 and hyperbranched polymer TM27-d to the reactor, stir for 1 hour to mix the materials evenly, cool the materials to below 30°C through circulating water, then add stabilizer HSCHEM-3200 and continue stirring for 10 minutes to mix the materials evenly; then cool the materials to below 30°C through circulating water, add mercaptan curing agent BrunoBock 330 and accelerator FXR-1020, stir for 1 hour to mix the materials evenly to obtain a single-component epoxy-thiol system adhesive. The obtained materials are divided into rubber cartridges and sealed to obtain finished products, which are stored at low temperatures below -20°C.
[0055] The one-component epoxy-thiol system adhesive was taken out from the storage cabinet at -20°C, placed at room temperature for 2 hours and then packaged. During the packaging process, the dispensing temperature was controlled between 20 and 30°C.
[0056] The encapsulation process is to first clean the surface of the substrate with non-woven cloth dipped in alcohol to remove dust and oil, and then apply glue to the joint between the two substrates to complete the encapsulation.
[0057] The encapsulated adhesive is heated at 80° C. for 10 to 30 minutes to complete curing. The mass fractions of each raw material in each embodiment and comparative example and the performance indicators of the final cured product are shown in Table 1.
[0058] Table 1
[0059]
[0060]
[0061] Comparative Example 1 is without adding core-shell resin, and it can be seen that the anti-drop ability is relatively poor, and it fails after 8 drops. Comparative Example 2 is with adding core-shell resin, and it can be seen that the anti-drop ability is significantly improved under the action of core-shell resin, and it can be dropped from 1.67 meters for more than 40 times without failure, but the zinc-nickel shear strength is slightly reduced (from 22.8 to 18.8).
[0062] Comparative Example 3 adds core-shell resin and hyperbranched polymer NJ292. It can be seen that the anti-drop ability is significantly improved under the action of the core-shell resin, and it can be dropped more than 40 times without failure at 1.67 meters. The zinc-nickel shear strength is also improved under the action of the hyperbranched polymer NJ292, but because the hyperbranched functional group does not match this glue system, the glue loses stability in storage. Comparative Example 4 adds core-shell resin and hyperbranched polymer H2M. It can be seen that the anti-drop ability is significantly improved under the action of the core-shell resin, and it can be dropped more than 40 times without failure at 1.67 meters; the zinc-nickel shear strength is also improved under the action of the hyperbranched polymer H2M, but because the hyperbranched functional group does not match this glue system, the glue loses stability in storage.
[0063] Comparative Examples 5 and 6 are added with hyperbranched polymer TM27-d. When no core-shell resin is added, the drop resistance is relatively poor. The shear strength of zinc-nickel is also improved under the action of hyperbranched polymer TM27-d. Since the hyperbranched functional groups matching this glue system are selected, the storage problem of the glue is improved (the standard is that the viscosity changes by <20% after being placed at room temperature for 7 days).
[0064] Examples 1 to 3 simultaneously add core-shell resin and specific hyperbranched polymer TM27-d, and have excellent comprehensive performance. Under the action of the core-shell resin, the product has good anti-drop ability and can fall from 1.67 meters for more than 40 times without failure. Compared with comparative example 2 without adding hyperbranched polymer TM-27d, the zinc-nickel shear strength is also significantly improved under the action of hyperbranched polymer TM-27d, and the storage stability is better than the formula adding other hyperbranched polymers.
[0065] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A one-component epoxy-thiol system adhesive, wherein: The adhesive comprises the following raw materials in parts by weight: The hyperbranched polymer is a polyolefin having anhydride groups as terminal groups.
2. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The anhydride group is succinic anhydride.
3. The one-component epoxy-thiol system adhesive according to claim 2, wherein: The hyperbranched polymer is obtained by reacting 3-allyl-cyclooctene and itaconic anhydride under the action of a Grubbs catalyst.
4. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, novolac epoxy resin and alicyclic epoxy resin.
5. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The core of the core-shell resin is selected from butadiene, butyl acrylate, Si, styrene or rubber, and the shell is selected from acrylics, styrene (ST), acrylonitrile (AN) and reactive monomers.
6. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The curing agent is a thiol curing agent, selected from at least one of trimethylolpropane tris(3-mercaptopropionate), 1,4-butanediol di(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), ethylene glycol di(3-mercaptopropionate), trimercaptothiol, tetrafunctional secondary thiol PE1, and polythiol.
7. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The accelerator is a latent accelerator, and is selected from at least one of FXR-1020, FXR-1030, FXR-1081, PN-23, PN-40, MY-24, EH-4337S, and EH-4360S.
8. The one-component epoxy-thiol system adhesive according to claim 1, wherein: The stabilizer is selected from at least one of ICAM-8401, ICAM-8402, HSCHEM-3200, and NP-100.
9. A method for preparing the one-component epoxy-thiol system adhesive according to any one of claims 1 to 8, wherein: The preparation method comprises the following steps: The epoxy resin, the hyperbranched polymer, the core-shell resin, the stabilizer, the curing agent and the accelerator are uniformly mixed to obtain the one-component epoxy-thiol system adhesive.
10. The preparation method according to claim 9, wherein: The preparation method specifically comprises the following processes: The epoxy resin, the hyperbranched polymer and the core-shell resin are added into the reactor, and stirred for 1 to 2 hours to mix evenly; after cooling the materials to below 30° C., a stabilizer is added and stirring is continued for 10 to 30 minutes; the materials are cooled to below 30° C. again, and then a curing agent and an accelerator are added, and stirred for 1 to 2 hours to mix evenly, so as to obtain the one-component epoxy-thiol system adhesive.
11. The preparation method according to claim 9 or 10, wherein: The preparation method further comprises: packaging the obtained one-component epoxy-thiol system adhesive into a rubber cartridge and sealing the cartridge to obtain a finished product, wherein the finished product is stored at a low temperature below -20°C.