Glass reinforced UV (ultraviolet) adhesive as well as preparation method and application thereof
Through the use of specific combinations of polyurethane acrylates and epoxy resins, as well as nanosilicon dioxide and polyacrylonitrile, the problems of insufficient adhesion and slow curing speed on the glass surface are solved, and high adhesion, strength and Fast curing glass-reinforced UV adhesives are suitable for a variety of high-precision and high-demand applications.
Patent Information
- Application Number
- CN202411441458.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional UV glue lacks adhesion on hard and smooth surfaces such as glass, has low bonding strength, is prone to falling off and cracking, and has a slow curing speed, which affects product stability and production efficiency.
Using a specific combination of oligomers and epoxy resins, including two polyurethane acrylates and two epoxy resins, the complex crosslinking network structure is formed through synergistic action, improving bond strength and curing speed, and using nanosilicon dioxide and polyacrylonitrile act as fillers to adjust viscosity and compatibility and reduce shrinkage.
It significantly improves the adhesion and bonding strength between UV glue and glass substrate, shortens the curing time, reduces the shrinkage rate, enhances stability and mechanical properties, and is suitable for optical, electronic, construction and automobile fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a glass-reinforced UV adhesive and a preparation method and application thereof. Background Art
[0002] With the rapid development of modern science and technology, UV glue (ultraviolet curing glue) has been widely used in the fields of electronics, optics, medical treatment, aerospace, etc. due to its advantages such as fast curing speed, easy operation, environmental protection and pollution-free. Especially in occasions requiring high-strength and high-precision bonding, UV glue has shown its unique advantages. However, with the continuous expansion of application scenarios, traditional UV glue has been unable to meet the diversified needs of the market in some aspects.
[0003] Traditional UV glue often has the problem of insufficient adhesion when applied to certain specific substrates, especially hard and smooth surfaces such as glass. This leads to unsatisfactory bonding effect, low bonding strength with the substrate, and easy to fall off and crack, which seriously affects the stability and service life of the product. UV glue often shrinks during the curing process, causing deformation and dimensional changes in the bonded parts. This not only affects the accuracy and performance of the product, but may also pose a safety hazard to the use of the product. Especially in applications with strict requirements on dimensional stability, such as the bonding of precision optical components, high shrinkage is a problem that needs to be solved urgently. In addition, on the production line, the curing speed of traditional UV glue still appears to be slow, which reduces production efficiency and increases production costs.
[0004] Therefore, it is necessary to develop a glass-reinforced UV adhesive that not only has excellent adhesion to the glass substrate and improves the bonding strength between glass and glass, but also has a fast curing speed, low shrinkage and good stability. Summary of the invention
[0005] The purpose of the present invention is to provide a glass-reinforced UV adhesive and a preparation method and application thereof. The glass-reinforced UV adhesive not only has excellent adhesion to a glass substrate and improves the bonding strength between glass and glass, but also has a fast curing speed, low shrinkage rate and good stability, and can be applied to the fields of optics, electronics, construction and automobiles.
[0006] In order to achieve the above object, the present invention provides the following technical solutions: A glass-reinforced UV adhesive, wherein the raw materials for its preparation include, by weight, 30-50 parts of oligomer, 20-40 parts of epoxy resin, 40-60 parts of active monomer, 5-10 parts of photoinitiator, 1-5 parts of auxiliary agent and 10-20 parts of filler.
[0007] Preferably, the oligomer includes a first urethane acrylate and a second urethane acrylate.
[0008] Preferably, the mass ratio of the first polyurethane acrylate to the second polyurethane acrylate is (2-4):1; more preferably, it is 3:1.
[0009] Preferably, the hydroxyl value of the first polyurethane acrylate is 145~155mgKOH / g, the viscosity is 1300~1500cp, the difunctionality, and the polymer content is 65%~75%; further preferably, the hydroxyl value of the first polyurethane acrylate is 150mgKOH / g, the viscosity is 1400cp, the difunctionality, and the polymer content is 70%.
[0010] In some preferred embodiments, the first polyurethane acrylate is purchased from Shanghai Zhenlishi Network Technology Co., Ltd. Zhanxin EBECRYL 8213.
[0011] Preferably, the second polyurethane acrylate has a molecular weight of 860, a viscosity of 300-700 cp, a functionality of 6, and a solid content of 100%.
[0012] In some preferred embodiments, the second polyurethane acrylate is purchased from Guangdong Xidun New Material Technology Co., Ltd. QDSRAYS UV063.
[0013] The inventors found that the use of two specific polyurethane acrylates as oligomers can shorten the curing speed of UV glue while improving the bonding strength between UV glue and glass substrate. This may be due to the synergistic effect between the two. On the one hand, the difference in the number of functional groups enables the two to form a network structure with different crosslinking densities during the curing process. The difunctional polyurethane acrylate helps to form stable crosslinking points, while the hexafunctional polyurethane acrylate can significantly increase the crosslinking density, thereby enhancing the curing effect and mechanical properties of the UV glue. On the other hand, the difference in viscosity allows the overall viscosity of the UV glue to be adjusted after the two are mixed, so that it has good fluidity and is easy to cure, which helps the wetting and penetration of the UV glue on the glass surface, thereby improving the bonding effect after curing. In addition, the use of low-functionality polyurethane acrylate can also reduce the shrinkage rate of UV glue. Polyurethane acrylate itself has good weather resistance and chemical resistance, and the mixed use of the two can further enhance these properties, thanks to the tightly crosslinked network structure they form, which can resist the erosion of harsh environments and chemicals. However, too high a functionality may also cause the curing reaction to be too violent and difficult to control, and may even cause side effects, such as increased shrinkage or increased internal stress, and may also lead to stress concentration at the bonding interface, which in turn reduces the bonding performance. The lower the functionality in the system, the fewer active groups there are, which reduces the cross-linking reaction speed and, in turn, the curing speed. However, only polyurethane acrylate oligomers can only improve the performance of UV adhesives to a limited extent.
[0014] Preferably, the epoxy resin includes bisphenol A epoxy resin and aliphatic epoxy resin.
[0015] Preferably, the mass ratio of the bisphenol A epoxy resin to the aliphatic epoxy resin is (1-3):1; more preferably, it is 2:1.
[0016] Preferably, the bisphenol A epoxy resin has an epoxy equivalent of 450-500 g / eq, a viscosity of 100-180 mPa·s, and a density of 1.18 g / cm3.
[0017] In some preferred embodiments, the epoxy resin is Nan Ya NPES-301 bisphenol A epoxy resin.
[0018] Preferably, the aliphatic epoxy resin has an epoxy equivalent of 305-335 g / eq, a viscosity of 3500-8000 mPa·s, and a density of 1.06 g / cm3.
[0019] In some preferred embodiments, the epoxy resin is Nan Ya NPER 032 aliphatic epoxy resin.
[0020] The inventor found that the selection of two specific epoxy resins can improve the curing speed of UV glue and further improve the adhesion of UV glue, especially for the adhesion of non-porous materials such as glass substrate. This may be because on the one hand, bisphenol A epoxy resin and aliphatic epoxy resin have differences in chemical structure, but both have reactive epoxy groups and can participate in curing reaction. By mixing, a more complex cross-linked network structure can be formed, thereby improving the cross-linking density of UV glue, and then improving the adhesion between UV glue and glass substrate, and different reactivity can accelerate the process of curing reaction, thereby improving the curing speed and curing effect of UV glue. In addition, bisphenol A epoxy resin has higher strength and hardness, while aliphatic epoxy resin has better flexibility and impact resistance. The mixed use of the two can balance the rigidity and flexibility of UV glue, so that it has both sufficient strength and certain toughness. Aliphatic epoxy resin can also reduce the viscosity of bisphenol A epoxy resin, improve the contact surface between UV glue and glass substrate, thereby improving bonding strength.
[0021] There is a certain synergistic effect between polyurethane acrylate and epoxy resin. On the one hand, the functional groups of polyurethane acrylate and bisphenol A epoxy resin and aliphatic epoxy resin can react chemically to form chemical bonds, which significantly improves the cohesion and adhesion of UV glue, and thus greatly improves the bonding strength and peel strength of UV glue. On the other hand, by mixing polyurethane acrylate with bisphenol A epoxy resin and aliphatic epoxy resin, a more complex and dense cross-linked network structure can be formed, which can more effectively disperse and withstand external forces, thereby improving the mechanical properties and durability of UV glue.
[0022] Preferably, the active monomer includes one or more of isobornyl methacrylate, hexanediol diacrylate, trimethylolpropane triacrylate, hydroxyethyl methacrylate, 4-hydroxybutyl vinyl ether, trivinyl glycol divinyl ether, and vinyl isobutyl ether; further preferably, it is hydroxyethyl methacrylate, isobornyl methacrylate, trimethylolpropane triacrylate, and trivinyl glycol divinyl ether.
[0023] Preferably, the mass ratio of hydroxyethyl methacrylate, isobornyl methacrylate, trimethylolpropane triacrylate and triethylene glycol divinyl ether is (1-3):(1-3):1:(2-4); more preferably, it is 2:2:1:3.
[0024] The inventors have found that the selection of specific active monomers can improve the curing speed of UV glue and the adhesion between the UV glue and the substrate, while also improving its yellowing resistance and transparency. This may be because on the one hand, hydroxyethyl methacrylate, isobornyl methacrylate and trimethylolpropane triacrylate are compounded to increase the crosslinking density of the polymer network while improving the curing speed of the UV glue, thereby improving the curing speed of the UV glue and the adhesion between the UV glue and the substrate. On the other hand, trivinyl glycol divinyl ether and the first three acrylate monomers are compounded, and both have excellent compatibility and reactivity, and can form a polymer network with excellent optical properties, thereby improving the transparency and yellowing resistance of the UV glue, and expanding the application range of the UV glue.
[0025] Preferably, the photoinitiator includes 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, benzoin, benzoin ethyl ether, benzoin dimethyl ether, benzophenone, bis(4-(diphenylsulfonium)phenyl)sulfide-bis(hexafluorophosphate); further preferably, 2-hydroxy-2-methyl-1-phenylpropanone, benzophenone, bis(4-(diphenylsulfonium)phenyl)sulfide-bis(hexafluorophosphate).
[0026] Preferably, the mass ratio of the 2-hydroxy-2-methyl-1-phenylpropanone, benzophenone, and bis(4-(diphenylsulfonium)phenyl)sulfide-bishexafluorophosphate is (4-6):(1-2):(1-3); more preferably, it is 5:1:2.
[0027] Preferably, the auxiliary agent is one or more of an adhesion promoter, a defoamer, a leveling agent, a wetting agent, and an antioxidant.
[0028] Preferably, the filler is modified nano-silicon dioxide and modified polyacrylonitrile.
[0029] Preferably, the mass ratio of the modified nano-silica to the modified polyacrylonitrile is 1:(0.5-2); further preferably, it is 1:1.
[0030] The inventors have found that the use of nano-silicon dioxide and polyacrylonitrile as fillers in UV glue can reduce the shrinkage of UV glue and improve its adhesion. This may be due to the synergistic effect of the two. Nano-silicon dioxide exists in the UV glue in the form of nano-chains, and is interwoven with polyacrylonitrile molecular chains to form a physical cross-linked network structure. This structure can not only enhance the internal strength of the UV glue and reduce the volume shrinkage during the curing process, but also improve the adhesion between the UV glue and the substrate, because the polar groups on the polyacrylonitrile molecular chains can form chemical bonds or hydrogen bonds with the surface of the substrate. However, nano-silicon dioxide is easy to agglomerate, and the compatibility between the two and the resin is poor, which affects its effect.
[0031] The preparation method of the modified nano silicon dioxide comprises the following steps: S1. After nano-silica is dispersed evenly in an ethanol aqueous solution, a silane coupling agent is added, and the mixture is stirred at 60-70° C. for 4-6 hours, centrifuged, washed with deionized water for 2-3 times, and dried to obtain substance 1; S2, after ultrasonication, add substance 1 and 2-bromoisobutyryl bromide to anhydrous triethylamine and tetrahydrofuran, react at room temperature for 20-30 hours, centrifuge, wash with deionized water 2-3 times, and dry to obtain substance 2; S3. After the substance II, methyl methacrylate, pentamethyldiethylenetriamine and dimethyl sulfoxide are evenly dispersed, cuprous bromide is added, and the mixture is reacted at 100-110°C for 7-12 minutes. Anhydrous ethanol is added until no precipitation is generated, and the mixture is centrifuged and washed with deionized water for 2-3 times to obtain modified nano-silica.
[0032] Preferably, the nano-silicon dioxide includes a first nano-silicon dioxide, a second nano-silicon dioxide, and a third nano-silicon dioxide.
[0033] Preferably, the mass ratio of the first nano-silicon dioxide, the second nano-silicon dioxide, and the third nano-silicon dioxide is (4-6):(2-4):1; more preferably, it is 5:3:1.
[0034] Preferably, the average particle size of the first nano-silica is 10~20nm, the specific surface area is 240~260m2 / g, and the loose density is 0.1~0.15g / cm3; further preferably, the average particle size of the first nano-silica is 15nm, the specific surface area is 250m2 / g, and the loose density is 0.1~0.15g / cm3.
[0035] Preferably, the average particle size of the second nano-silica is 25~35nm, the specific surface area is 190~210m2 / g, and the loose density is 0.15~0.18g / cm3; further preferably, the average particle size of the second nano-silica is 30nm, the specific surface area is 200m2 / g, and the loose density is 0.15~0.18g / cm3.
[0036] Preferably, the third nano-silicon dioxide has an average particle size of 60 nm, a specific surface area of 150-200 m2 / g, and a loose density of 0.18-0.2 g / cm3.
[0037] In some preferred embodiments, the nano-silicon dioxide is purchased from Beijing Dekedaojin Technology Co., Ltd.
[0038] Preferably, the volume concentration of ethanol in the ethanol aqueous solution is 60% to 70%.
[0039] Preferably, the mass ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1:20-30.
[0040] Preferably, the silane coupling agent is a mixture of γ-aminopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane.
[0041] Preferably, the mass ratio of γ-aminopropyltriethoxysilane to γ-mercaptopropyltrimethoxysilane is (1-3):1; more preferably, it is 2:1.
[0042] Preferably, the added amount of the silane coupling agent is 10% to 20% of the mass of the nano-silicon dioxide.
[0043] Preferably, the mass ratio of the anhydrous triethylamine, substance 1, and 2-bromoisobutyryl bromide is (3-5):(1-3):(2-4); more preferably, it is 4:2:3.
[0044] Preferably, the mass ratio of anhydrous triethylamine to tetrahydrofuran is 1:(20-30); further preferably, it is 1:25.
[0045] Preferably, the mass ratio of the second substance to methyl methacrylate is 1:(5-8); further preferably, it is 1:6.
[0046] Preferably, the mass of the dimethyl sulfoxide is 40 to 50 times that of substance 2.
[0047] Preferably, the total mass of pentamethyldiethylenetriamine and cuprous bromide is 15% to 25% of the mass of substance 2.
[0048] Preferably, the mass ratio of pentamethyldiethylenetriamine to cuprous bromide is (1-2):1; more preferably, it is 3:2.
[0049] The inventors found that by selecting three nano-silicon dioxides with different particle sizes, first modifying their surfaces with a specific silane coupling agent, and then polymerizing on their surfaces to form a polymethyl methacrylate chain structure, the dispersibility and stability of the modified nano-silicon dioxide can be improved while also improving its compatibility with UV resin, thereby improving the performance of UV glue. This may be because nano-silicon dioxides with different particle sizes fill each other to form smaller gaps, making the dispersion of nanoparticles in the matrix more uniform, and the active groups on their surfaces and molecular chains may produce strong interactions to form stronger interfacial bonding forces, thereby enhancing the overall performance of UV glue, and nano-silicon dioxide can play a stress concentration role in the matrix, triggering silver streaks and absorbing energy, preventing silver streaks from developing into destructive cracks, thereby improving the toughness of UV glue. Nano-silicon dioxide has a large number of active silicon groups on its surface. Surface modification of nano-silicon dioxide with a specific silane coupling agent can change the chemical properties of its surface, introduce new functional groups, and reduce the number of hydroxyl groups on its surface, thereby reducing its hydrophilicity and improving its dispersibility and stability in the system. Secondly, the modified nano-silica surface is polymerized to form a polymethyl methacrylate chain structure, which combines the organic polymer chain with the inorganic nanoparticles through chemical bonds to form a nano-composite material with a core-shell structure. This structure not only improves the compatibility of nano-silica in UV resin, but also enables it to be more effectively dispersed in the resin matrix, thereby reducing the agglomeration of nanoparticles. Finally, due to the introduction of the polymethyl methacrylate chain structure, the interaction between the nano-composite material and the UV resin is enhanced, thereby jointly improving the interfacial bonding force between the nano-composite material and the UV resin, which helps to improve the performance of the UV adhesive and improve its adhesion, strength and heat resistance. However, its addition amount should not be too much.
[0050] The preparation method of the modified polyacrylonitrile comprises the following steps: A1. Dissolve polymethyl methacrylate in N,N-dimethylformamide, stir at room temperature for 1-2 days, and remove bubbles by ultrasonic to obtain solution 1; A2, dissolving polyacrylonitrile in N,N-dimethylformamide, stirring at room temperature for 1-2 days, and removing bubbles by ultrasonication to obtain solution 2; A3. With solution 1 as the shell layer and solution 2 as the core layer, a nanofiber membrane was obtained by coaxial electrospinning. The nanofiber membrane was sheared at 10,000-20,000 r / min for 20-30 min to obtain modified polyacrylonitrile.
[0051] Preferably, the polymethyl methacrylate has an average molecular weight of 15,000 and is purchased from Merck Chemical.
[0052] Preferably, the average molecular weight of the polyacrylonitrile is 150,000 and is purchased from Merck Chemical.
[0053] Preferably, the mass ratio of polymethyl methacrylate to N,N-dimethylformamide is 1:(5-7); more preferably, it is 1:6.
[0054] Preferably, the mass ratio of polyacrylonitrile to N,N-dimethylformamide is 1:(7-9); further preferably, it is 1:8.
[0055] Preferably, the flow rate of solution one is 1.5 to 2 times the flow rate of solution two, and the flow rate is used to control the amount of solution one and solution two added to ensure that solution one and solution two are used up after the reaction is completed.
[0056] In some preferred schemes, after PMMA is modified with polyacrylonitrile, not only the functional groups on its surface may chemically react with the resin molecules in the UV glue to form chemical bonds, thereby improving the adhesion between the UV glue and the substrate, but also the nanofiber structure of PMMA-modified polyacrylonitrile can enhance the internal structural strength of the UV glue, giving it higher tensile strength and toughness.
[0057] The preparation method of the glass-reinforced UV adhesive comprises the following steps: mixing the raw materials evenly.
[0058] The glass-enhanced UV adhesive can be applied to glass furniture, construction and automobile glass, optical instruments and other fields.
[0059] Compared with the prior art, the advantages and beneficial effects of the present invention are: 1. The present invention provides a glass-reinforced UV adhesive, which not only has excellent adhesion to the glass substrate and improves the bonding strength between glass and glass, but also has a fast curing speed, low shrinkage rate, and good stability, and has a wide range of application value in the fields of optics, electronics, construction, and automobiles.
[0060] 2. The present invention selects two specific polyurethane acrylates as oligomers, which can shorten the curing speed of the UV glue and improve the bonding strength between the UV glue and the glass substrate.
[0061] 3. The present invention can increase the curing speed of UV glue by selecting two specific epoxy resins, and further improve the adhesion of UV glue, especially the adhesion to non-porous materials such as glass substrates.
[0062] 4. The present invention can improve the curing speed of UV glue and the adhesion between the UV glue and the substrate by selecting specific active monomers, while also improving its yellowing resistance and transparency.
[0063] 5. The present invention selects nano silicon dioxide and polyacrylonitrile as fillers for use in UV glue, which can reduce the shrinkage rate of UV glue and improve its adhesion.
[0064] 6. The present invention selects three nano-silica with different particle sizes, first modifies their surfaces with a specific silane coupling agent, and then polymerizes them on the surface to form a polymethyl methacrylate chain structure, which can improve the dispersibility and stability of the modified nano-silica while also improving its compatibility with UV resin, thereby improving the performance of UV glue. DETAILED DESCRIPTION
[0065] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0066] The raw materials used in the present invention are all commercially available, specifically: The first polyurethane acrylate, with a hydroxyl value of 150 mgKOH / g, a viscosity of 1400 cp, difunctionality, and a polymer content of 70%, was purchased from Shanghai Zhenlishi Network Technology Co., Ltd. Zhanxin EBECRYL 8213.
[0067] The second polyurethane acrylate, with a molecular weight of 860, a viscosity of 300-700 cp, a functionality of 6, and a solid content of 100%, was purchased from Guangdong Xidun New Materials Technology Co., Ltd. QDSRAYS UV063.
[0068] The epoxy equivalent of bisphenol A epoxy resin is 450~500g / eq, the viscosity is 100~180mPa·s, and the density is 1.18g / cm 3 , Nan Ya NPES-301 bisphenol A epoxy resin.
[0069] The epoxy equivalent of aliphatic epoxy resin is 305~335g / eq, the viscosity is 3500~8000mPa·s, and the density is 1.06g / cm 3, Nan Ya NPER 032 aliphatic epoxy resin.
[0070] Adhesion promoter, Changxing Chemical, EM39.
[0071] Defoaming agent, Defeng DF-10.
[0072] Leveling agent, BYK, BYK333.
[0073] The average particle size of the first nano-silicon dioxide is 15nm and the specific surface area is 250m 2 / g, bulk density is 0.1~0.15g / cm 3 The average particle size of the second nano-silicon dioxide is 30nm and the specific surface area is 200m 2 / g, bulk density is 0.15~0.18g / cm 3 ; The average particle size of the third nano-silicon dioxide is 60nm, and the specific surface area is 150~200m 2 / g, bulk density is 0.18~0.2g / cm 3 ; All purchased from Beijing Dekedaojin Technology Co., Ltd.
[0074] Polymethyl methacrylate has an average molecular weight of 15,000 and was purchased from Merck Chemicals.
[0075] Polyacrylonitrile has an average molecular weight of 150,000 and was purchased from Merck Chemicals.
[0076] Example 1. This example provides a glass-reinforced UV adhesive. The raw materials for its preparation, measured by weight, include 40 parts of oligomer, 30 parts of epoxy resin, 50 parts of active monomer, 8 parts of photoinitiator, 3 parts of auxiliary agent, and 15 parts of filler.
[0077] The oligomer is a first polyurethane acrylate and a second polyurethane acrylate, and the mass ratio is 3:1.
[0078] The epoxy resin is bisphenol A epoxy resin and aliphatic epoxy resin, and the mass ratio is 2:1.
[0079] The active monomers are hydroxyethyl methacrylate, isobornyl methacrylate, trimethylolpropane triacrylate, and trivinyl glycol divinyl ether, and the mass ratio is 2:2:1:3.
[0080] The photoinitiator is 2-hydroxy-2-methyl-1-phenylacetone, benzophenone, and bis(4-(diphenylsulfonium)phenyl)sulfide-bishexafluorophosphate, and the mass ratio is 5:1:2.
[0081] The auxiliary agents are adhesion promoter, defoamer, leveling agent and wetting agent, and the mass ratio is 5:1:1:1.
[0082] The filler is modified nano silicon dioxide and modified polyacrylonitrile, and the mass ratio is 1:1.
[0083] The preparation method of the modified nano silicon dioxide comprises the following steps: S1. After nano-silica is dispersed evenly in an ethanol aqueous solution, a silane coupling agent is added, and the mixture is stirred at 65° C. for 5 h, centrifuged, washed twice with deionized water, and dried to obtain substance 1; S2, after ultrasonication, add substance 1 and 2-bromoisobutyryl bromide to anhydrous triethylamine and tetrahydrofuran, react at room temperature for 25 hours, centrifuge, wash twice with deionized water, and dry to obtain substance 2; S3. After the substance II, methyl methacrylate, pentamethyldiethylenetriamine and dimethyl sulfoxide are uniformly dispersed, cuprous bromide is added, and the mixture is reacted at 105° C. for 10 min. Anhydrous ethanol is added until no precipitation is generated, and the mixture is centrifuged and washed twice with deionized water to obtain modified nano-silica.
[0084] The nano silicon dioxide includes first nano silicon dioxide, second nano silicon dioxide and third nano silicon dioxide, and the mass ratio is 5:3:1.
[0085] The volume concentration of ethanol in the ethanol aqueous solution is 65%.
[0086] The mass ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1:25.
[0087] The silane coupling agent is γ-aminopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane, and the mass ratio is 2:1.
[0088] The added amount of the silane coupling agent is 15% of the mass of the nano-silicon dioxide.
[0089] The mass ratio of the anhydrous triethylamine, substance 1, and 2-bromoisobutyryl bromide is 4:2:3.
[0090] The mass ratio of the anhydrous triethylamine to tetrahydrofuran is 1:25.
[0091] The mass ratio of the second substance to methyl methacrylate is 1:6.
[0092] The mass of the dimethyl sulfoxide is 45 times that of substance 2.
[0093] The total mass of the pentamethyldiethylenetriamine and cuprous bromide is 20% of the mass of substance 2.
[0094] The mass ratio of pentamethyldiethylenetriamine to cuprous bromide is 3:2.
[0095] The preparation method of the modified polyacrylonitrile comprises the following steps: A1, dissolving polymethyl methacrylate in N,N-dimethylformamide, stirring at room temperature for 1 day, and removing bubbles by ultrasonication to obtain solution 1; A2, dissolving polyacrylonitrile in N,N-dimethylformamide, stirring at room temperature for 1 day, and removing bubbles by ultrasonication to obtain solution 2; A3. With solution 1 as the shell layer and solution 2 as the core layer, a nanofiber membrane was obtained by coaxial electrospinning. The nanofiber membrane was sheared at 150,000 r / min for 25 min to obtain modified polyacrylonitrile.
[0096] The mass ratio of the polymethyl methacrylate to N,N-dimethylformamide is 1:6.
[0097] The mass ratio of the polyacrylonitrile to N,N-dimethylformamide is 1:8.
[0098] The flow rate of solution one is 1.8 times that of solution two, and the flow rate is used to control the addition amount of solution one and solution two to ensure that solution one and solution two are used up after the reaction is completed.
[0099] The preparation method of the glass-reinforced UV adhesive comprises the following steps: mixing the raw materials evenly.
[0100] Embodiment 2: The difference between this embodiment and embodiment 1 is that the oligomer is a first polyurethane acrylate and a second polyurethane acrylate, and the mass ratio is 2:1.
[0101] Embodiment 3: The difference between this embodiment and embodiment 1 is that the nano-silicon dioxide comprises a first nano-silicon dioxide, a second nano-silicon dioxide, and a third nano-silicon dioxide, and the mass ratio is 1:1:1.
[0102] Comparative Example 1: The difference between this comparative example and Example 1 is that the oligomer is a first polyurethane acrylate.
[0103] Comparative Example 2: The difference between this comparative example and Example 1 is that the oligomer is a first polyurethane acrylate and a second polyurethane acrylate, and the mass ratio is 1:1.
[0104] Comparative Example 3: The difference between this comparative example and Example 1 is that the epoxy resin is bisphenol A type epoxy resin.
[0105] Comparative Example 4: The difference between this comparative example and Example 1 is that the epoxy resin is bisphenol A epoxy resin and aliphatic epoxy resin, and the mass ratio is 1:2.
[0106] Comparative Example 5: The difference between this comparative example and Example 1 is that the active monomers are hydroxyethyl methacrylate, isobornyl methacrylate, and trivinyl glycol divinyl ether in a mass ratio of 2:2:3.
[0107] Comparative Example 6: The difference between this comparative example and Example 1 is that the filler is nano-silicon dioxide and polyacrylonitrile, and the mass ratio is 1:1.
[0108] Comparative Example 7: The difference between this comparative example and Example 1 is that the nano-silicon dioxide is the first nano-silicon dioxide.
[0109] Comparative Example 8, the difference between this comparative example and Example 1 is: the preparation method of the modified nano-silica comprises the following steps: after the nano-silica is evenly dispersed in an ethanol aqueous solution, a silane coupling agent is added, the mixture is stirred at 65°C for 5 hours, centrifuged, washed twice with deionized water, and dried.
[0110] Comparative Example 9: The difference between this comparative example and Example 1 is that the raw materials for preparing the glass reinforced UV adhesive, calculated by weight, include 70 parts of oligomers, 50 parts of active monomers, 8 parts of photoinitiators, 3 parts of additives, and 15 parts of fillers.
[0111] Performance Testing Refer to GB 1728-79 to test the curing time, the glue thickness is 200μm, the room temperature is about 25℃, the portable UV curing machine provides 250W ultraviolet light irradiation, the lamp distance is 4cm, there is no adhesive on the finger, that is, the surface is considered dry, and the measurement unit is s. Refer to GB / T 2790-1995 to test the peel strength of UV glue, the substrate is two glass plates. According to GB / T 9286-88, the adhesion of UV glue after curing is measured, which is divided into 6 levels (0-5), with level 0 being the best and level 5 being the worst. The volume shrinkage rate is obtained by dividing the volume difference before and after curing by the liquid volume before curing. The results are shown in Table 1.
[0112]
[0113] According to statistics, the glass-reinforced UV adhesive prepared by Examples 1 to 3 of the present invention has a long curing time period, high peel strength, high adhesion to the glass substrate, and low shrinkage. Comparative Example 1 does not add the second polyurethane acrylate, Comparative Example 2 adds too much second polyurethane acrylate, Comparative Example 3 does not add aliphatic epoxy resin, Comparative Example 4 adds too much aliphatic epoxy resin, Comparative Example 5 does not add trimethylolpropane triacrylate, Comparative Example 6 does not modify nano-silicon dioxide and polyacrylonitrile, Comparative Example 7 does not add the second nano-silicon dioxide and the third nano-silicon dioxide, Comparative Example 8 does not polymerize on the surface of silicon dioxide to form a polymethyl methacrylate chain structure, Comparative Example 9 does not add epoxy resin, and the prepared glass-reinforced UV adhesive has a long curing time, low peel strength and adhesion, and high shrinkage. Therefore, the glass-reinforced UV adhesive prepared by the raw materials and methods described in this application not only has excellent adhesion to the glass substrate, improves the bonding strength between glass and glass, but also has a fast curing speed, low shrinkage, and good stability, and shows a wide range of application value in the fields of optics, electronics, construction, and automobiles.
[0114] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A glass-reinforced UV adhesive, characterized in that: The raw materials for its preparation include 30-50 parts of oligomer, 20-40 parts of epoxy resin, 40-60 parts of active monomer, 5-10 parts of photoinitiator, 1-5 parts of auxiliary agent and 10-20 parts of filler by weight; the oligomer includes a first polyurethane acrylate and a second polyurethane acrylate; the first polyurethane acrylate has a hydroxyl value of 145-155 mgKOH / g, a viscosity of 1300-1500 cp, a difunctionality and a polymer content of 65%-75%; the second polyurethane acrylate has a molecular weight of 860, a viscosity of 300-700 cp, a functionality of 6 and a solid content of 100%; the epoxy resin includes a bisphenol A epoxy resin and an aliphatic epoxy resin; the bisphenol A epoxy resin has an epoxy equivalent of 450-500 g / eq, a viscosity of 100-180 mPa·s and a density of 1.18 g / cm 3 The epoxy equivalent of the aliphatic epoxy resin is 305-335 g / eq, the viscosity is 3500-8000 mPa·s, and the density is 1.06 g / cm 3 .
2. The glass-reinforced UV adhesive according to claim 1, characterized in that: The mass ratio of the first polyurethane acrylate to the second polyurethane acrylate is (2-4):
1.
3. The glass-reinforced UV adhesive according to claim 1, characterized in that: The mass ratio of the bisphenol A epoxy resin to the aliphatic epoxy resin is (1-3):
1.
4. The glass-reinforced UV adhesive according to claim 1, characterized in that: The active monomers include one or more of isobornyl methacrylate, hexanediol diacrylate, trimethylolacrylate tripropylene, hydroxyethyl methacrylate, 4-hydroxybutyl vinyl ether, trivinyl glycol divinyl ether, and vinyl isobutyl ether.
5. The glass-reinforced UV adhesive according to claim 1, characterized in that: The photoinitiator includes 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, benzoin, benzoin ethyl ether, benzoin dimethyl ether, benzophenone, and bis(4-(diphenylsulfonium)phenyl)sulfide-bishexafluorophosphate.
6. The glass-reinforced UV adhesive according to claim 1, characterized in that: The fillers are modified nano silicon dioxide and modified polyacrylonitrile.
7. The glass-reinforced UV adhesive according to claim 6, characterized in that: The preparation method of the modified nano silicon dioxide comprises the following steps: S1. After nano-silica is dispersed evenly in an ethanol aqueous solution, a silane coupling agent is added, and the mixture is stirred at 60-70° C. for 4-6 hours, centrifuged, washed with deionized water for 2-3 times, and dried to obtain substance 1; S2, after ultrasonication, add substance 1 and 2-bromoisobutyryl bromide to anhydrous triethylamine and tetrahydrofuran, react at room temperature for 20-30 hours, centrifuge, wash with deionized water 2-3 times, and dry to obtain substance 2; S3. After the substance II, methyl methacrylate, pentamethyldiethylenetriamine and dimethyl sulfoxide are evenly dispersed, cuprous bromide is added, and the mixture is reacted at 100-110°C for 7-12 minutes. Anhydrous ethanol is added until no precipitation is generated, and the mixture is centrifuged and washed with deionized water for 2-3 times to obtain modified nano-silica.
8. The method for preparing glass-reinforced UV adhesive according to claim 7, characterized in that: The nano silicon dioxide comprises a first nano silicon dioxide, a second nano silicon dioxide and a third nano silicon dioxide.
9. A method for preparing the glass-reinforced UV adhesive according to any one of claims 1 to 8, characterized in that: The steps are: mix the raw materials evenly.
10. Use of the glass-reinforced UV adhesive according to any one of claims 1 to 8 in the fields of glass furniture, building and automobile glass, and optical instruments.
Citation Information
Patent Citations
UV curing color decorative coating
CN101407651A
Synthesis and application of light-cured polyurethane-acrylic acid-epoxy resin adhesive
CN102079810A
Glass reinforced UV adhesive and preparation method thereof
CN104745140A
Photocurable adhesive, preparation method and application thereof
CN112126402A
UV light source cured glass roller coating adhesion primer and preparation method thereof