Transition-state binder, preparation method thereof and method for preparing high-strength carbon-containing pellets
Through the transitional binder with optimized proportion and cold press forming technology, the problems of deterioration and powderization during the roasting process of carbon-containing pellets are solved, and efficient hot and cold strength is achieved, and metallurgical performance is improved.
Patent Information
- Application Number
- CN202310629642.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, carbon-containing pellets have problems with deterioration in strength and severe powderization during roasting, especially before cold strength failure and high-temperature strength regeneration, it is difficult to meet the production requirements of high-efficiency reactors.
Using transitional binders with optimized ratios, including organic binders, bentonite, bauxite, limestone and phenolic resin, it is prepared by dry grinding, combined with cold pressing molding and drying treatment, high-strength carbon-containing pellets.
In the blast furnace iron smelting and direct reduction of carbon-containing pellets, the hot and cold strength of the pellets is improved, the metallurgical performance is improved, and the strength deterioration and powdering problems are solved.
Smart Images

Figure BDA0004257993660000021 
Figure BDA0004257993660000141 
Figure FDA0004257993650000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and relates to a transitional binder and a preparation method thereof, and a method for preparing high-strength carbon-containing pellets. Background Art
[0002] At present, the steel industry production is mainly based on the long process of blast furnace-converter, which has the characteristics of large scale, high efficiency and low cost. However, blast furnace production depends on high-quality coke, while the coking production process has high energy consumption, large pollutant emissions, and consumes expensive coking coal resources. Direct reduction ironmaking production technology has attracted the attention of many ironmaking producers because it has gotten rid of the dependence on expensive coking coal resources; among them, direct reduction ironmaking technology can be divided into two categories: gas-based direct reduction ironmaking technology and coal-based direct reduction ironmaking technology. The reducing agent of gas-based direct reduction ironmaking mainly includes H2, CO or other mixed gases, and its reaction vessels for producing direct reduction ironmaking include vertical furnaces, reaction tanks and fluidized beds, mainly including MIDREX method, HYL method, FIOR method, etc.; the reducing agent used in coal-based direct reduction is mainly coal, and its reaction vessels for reducing iron oxides include rotary kilns, rotary hearth furnaces, vertical furnaces and externally heated reaction tanks, mainly including DRC method, FASMET method, SL / RN method, etc.
[0003] Carbon-containing pellets have been widely used in ironmaking production processes due to their good reactivity and wide range of raw material applications. However, unlike iron ore concentrate pellets, carbon-containing pellets are added with a certain proportion of solid carbon reducing agent in the iron ore powder raw material, resulting in low strength of raw balls and dry balls. At the same time, during the high-temperature roasting process, the physical structure of the pellets changes due to the gasification reaction of carbon in the reducing agent, the reduction of iron oxides, and the multiple effects of thermal stress, causing the rapid decrease in the thermal strength of the pellets, making it difficult for carbon-containing pellets to meet the production requirements of efficient reactors. At present, there are studies at home and abroad on the use of rotary hearth furnace direct reduction process or similar processes to treat carbon-containing pellets to prepare metallized furnace charges. The reason for success is that the material layer of this type of process is relatively thin, generally only a single layer of furnace charge or several layers of furnace charge, and the furnace charge is in a relatively static state during the reduction process. The load of the pellets during the reduction process is low, and the requirements for the strength of the pellets are not high. Therefore, how to ensure the strength of the pellets has become the key to the development of efficient smelting carbon-containing pellets to prepare metallized furnace charge technology.
[0004] At present, there are few technologies for preparing high-strength carbon-containing pellets. For example, Chinese Patent Publication No. CN112575182A uses a hot pressing method to prepare red mud carbon-containing pellets; Chinese Patent Publication No. CN110129557A uses bituminous coal, lean coal, vanadium-titanium ore and vanadium-titanium sea sand ore as raw materials to prepare carbon-containing pellets by hot pressing; Chinese Patent Publication No. CN110079668A uses iron ore powder, coal powder and binder in different proportions to prepare double-layer carbon-containing pellets by two pelletizing processes; Chinese Patent Publication No. CN108504857A uses an inorganic binder, a regulator, a reducing agent and an iron-containing material to mix and prepare cold-consolidated carbon-containing pellets by cold pressing. Although the above-mentioned technology for preparing carbon-containing pellets can obtain high-strength carbon-containing pellets, there are problems such as high energy consumption, low production efficiency, and difficult-to-solve process pollutant emissions. Some researchers use organic binders to ensure the strength of cold pellets, and inorganic binders to ensure the strength in the high-temperature zone. However, in actual production, the cold strength fails between 400 and 1000°C, but the high-temperature thermal strength has not yet taken effect. Due to the lack of the use of transitional binders in this temperature range, the strength of the carbon-containing pellets deteriorates during the roasting process, and the problem of severe pulverization occurs.
[0005] By searching the prior art, no relevant reports have been found on the technology of producing high-strength carbon-containing pellets in the transition state binder. In view of this, it is urgent to study a binder with both cold and hot strength bonding effects, which can strengthen the strength of carbon-containing pellets before the cold strength fails and the high-temperature strength regenerates during the roasting process of carbon-containing pellets. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a transitional binder and a preparation method and a method for preparing high-strength carbon-containing pellets. By optimizing the ratio of the raw materials of the transitional binder, a transitional binder with both cold and hot strength bonding effects is obtained; the transitional binder can solve the problems of strength deterioration and severe pulverization of carbon-containing pellets in the roasting process of the prior art, and plays a role in strengthening the strength of carbon-containing pellets before the cold strength fails and the high-temperature strength regenerates during the blast furnace ironmaking and direct reduction ironmaking processes of the carbon-containing pellets.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides a transitional binder, the raw materials of which include the following components in parts by weight:
[0009]
[0010] Preferably, the burnout of the organic binder is ≥80%; and / or
[0011] The bentonite has an absorption capacity of ≥30%; and / or
[0012] The content of Al2O3 in the bauxite is ≥ 60wt%; and / or
[0013] The content of CaO in the limestone is ≥ 60%; and / or
[0014] The phenolic resin has a residual carbon rate of ≥50%; and / or
[0015] The viscosity of the pregelatinized starch is ≥700 mPa·s.
[0016] Preferably, the organic binder is one or more of paraffin beeswax, polyoxymethylene, polyvinyl alcohol, and acetic acid copolymer; and / or
[0017] The pregelatinized starch is one or more of corn pregelatinized starch, wheat pregelatinized starch, potato pregelatinized starch, cassava pregelatinized starch, and rice pregelatinized starch.
[0018] Preferably, the particle sizes of the organic binder, bauxite and limestone are all ≤5 mm.
[0019] The second aspect of the present invention provides a method for preparing a transitional binder as described in the first aspect of the present invention, characterized in that an organic binder, bentonite, bauxite, limestone, phenolic resin, and pregelatinized starch are mixed in proportion and stirred evenly to obtain a mixture, and the mixture is ground to a particle size of ≤0.1 mm by dry grinding to obtain a transitional binder.
[0020] A third aspect of the present invention provides a method for preparing high-strength carbon-containing pellets, comprising the following steps:
[0021] S1, mixing the transitional binder as described in the first aspect of the present invention with iron ore powder and reduced carbon in a certain proportion to obtain a mixture;
[0022] S2, adding water to the mixture, stirring and mixing, and then cold pressing to obtain carbon-containing wet pellets;
[0023] S3, drying the carbon-containing wet pellets to obtain high-strength carbon-containing pellets.
[0024] Preferably, in step S1:
[0025] The iron ore powder has a total iron content of ≥55wt%, an S content of ≤0.6wt%, and a P content of ≤0.1wt%; and / or
[0026] In the iron ore powder, the mass proportion of the part with a particle size of ≤0.074 is greater than 80%; and / or
[0027] The reduced carbon has a dry basis volatile matter content of ≤20wt%, a dry basis ash content of ≤15wt%, a dry basis fixed carbon content of ≥70wt%, and a dry basis S content of ≤0.5wt%; and / or
[0028] In the reduced carbon, the mass proportion of the part with a particle size of ≤0.074 is greater than 70%; and / or
[0029] The weight ratio of the transitional binder to the iron ore powder and the reduced carbon is 2-10:70-80:10-20.
[0030] Preferably, in step S1:
[0031] The iron ore powder includes one or a mixture of magnetite, hematite, limonite, goethite, and vanadium-iron magnetite; and / or
[0032] The reducing carbon includes one or a mixture of anthracite, bituminous coal, upgraded coal, semi-coke, biomass charcoal, pyrolytic carbon black, and coke powder.
[0033] Preferably, in step S2:
[0034] The amount of water added is 3-10 wt% of the mixture; and / or
[0035] The cold press forming pressure is 5 to 100 MPa; and / or
[0036] The carbon-containing wet pellets have a compressive strength of ≥150N / piece, a 0.5m drop strength of ≥3 times, and a thermal burst temperature of ≥500°C.
[0037] Preferably, the carbon-containing wet pellets have a 0.5 m drop strength of ≥ 4 times, and a thermal burst temperature of ≥ 730°C.
[0038] Preferably, in step S3:
[0039] The high-strength carbon-containing pellets have a compressive strength of ≥2000N / piece and a 0.5m drop strength of ≥15 times; and / or
[0040] The high-strength carbon-containing pellets calcined at 600°C have a high-temperature compressive strength of ≥1000N / piece and a 0.5m drop strength of ≥15 times; and / or
[0041] The high-strength carbon-containing pellets calcined at 900°C have a high-temperature compressive strength of ≥300N / piece and a 0.5m drop strength of ≥15 times; and / or
[0042] The high-strength carbon-containing pellets calcined at 1200°C have a high-temperature compressive strength of ≥2000N / piece, a 3m drop strength of ≥5 times, and a metallization rate of ≥80%.
[0043] Preferably, in step S3:
[0044] The high-strength carbon-containing pellets have a compressive strength of ≥2100N / piece and a 0.5m drop strength of ≥25 times; and / or
[0045] The high-strength carbon-containing pellets calcined at 600°C have a high-temperature compressive strength of 2500-3000N / piece and a 0.5m drop strength of ≥50 times; and / or
[0046] The high-temperature compressive strength of the high-strength carbon-containing pellets after calcination at 900°C is ≥600N / piece; and / or
[0047] The high-strength carbon-containing pellets calcined at 1200°C have a high-temperature compressive strength of ≥4000N / piece and a 3m drop strength of ≥10 times.
[0048] The transitional binder and preparation method thereof and the method for preparing high-strength carbon-containing pellets of the present invention have the following beneficial effects:
[0049] 1. Compared with the prior art, the present invention optimizes the ratio of the raw materials of the transitional binder to obtain a transitional binder with both cold and hot strength bonding effects; the transitional binder can solve the problems of strength degradation and severe pulverization during the roasting process of carbon-containing pellets in the prior art, and plays a role in strengthening the strength of carbon-containing pellets before the cold strength fails and the high-temperature strength regenerates during the blast furnace ironmaking and direct reduction ironmaking processes of carbon-containing pellets;
[0050] 2. The transitional binder prepared by the present invention has a wide source of raw materials, low price, and has the effect of direct bonding with both cold and hot strengths. It can improve the cold and hot strength of carbon-containing pellets and improve the metallurgical properties of carbon-containing pellets. DETAILED DESCRIPTION
[0051] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with embodiments.
[0052] The transition state binder provided by the present invention comprises the following raw materials in parts by weight: 20-80 parts of organic binder, 5-40 parts of bentonite, 2-10 parts of bauxite, 2-20 parts of limestone, 2-20 parts of phenolic resin and 5-30 parts of pregelatinized starch.
[0053] The quality indicators and design principles of each component of the raw materials in the transitional binder are as follows:
[0054] Organic binder: burnout ≥ 80%; in the transitional binder, the organic binder mainly plays a role in improving the low-temperature roasting strength of the carbon-containing pellets; in a further specific embodiment, the organic binder can be one or more of paraffin, beeswax, polyoxymethylene, polyvinyl alcohol, and acetic acid copolymer;
[0055] Bentonite: Blue absorption ≥ 30%; in the transitional binder, bentonite mainly plays a role in improving the balling performance of the pellets, enhancing the raw ball strength, and increasing the balling rate;
[0056] Bauxite: Al2O3 content ≥ 60wt%; in the transitional binder, bauxite mainly plays a role in improving the high temperature roasting strength of carbon-containing pellets;
[0057] Limestone: CaO content ≥ 60%; in the transitional binder, limestone mainly plays the role of improving carbon-containing pellets, adjusting the basicity of carbon-containing pellets, and improving the high-temperature roasting strength of carbon-containing pellets;
[0058] Phenolic resin: residual carbon rate ≥50%; in the transitional binder, phenolic resin mainly plays a role in improving the high temperature roasting strength of carbon-containing pellets;
[0059] The viscosity of the pregelatinized starch is ≥700mPa·s; in the transitional binder, the pregelatinized starch mainly plays a role in improving the strength of raw and dried carbon-containing pellets; in a further specific embodiment, the pregelatinized starch can be one or more of corn pregelatinized starch, wheat pregelatinized starch, potato pregelatinized starch, cassava pregelatinized starch, and rice pregelatinized starch.
[0060] In order to ensure that the various components of the transitional binder can be fully mixed, the particle sizes of the organic binder, bauxite and limestone are all ≤5mm.
[0061] The present invention also provides a method for preparing a transitional binder, comprising mixing an organic binder, bentonite, bauxite, limestone, phenolic resin and pregelatinized starch in proportion and stirring to obtain a mixture, and grinding the mixture to a particle size of ≤0.1 mm by dry grinding to obtain the transitional binder.
[0062] The specific process of the preparation method of the above-mentioned transition state binder is as follows:
[0063] (1) Select raw materials according to the components and quality indicators of the transitional binder, namely, organic binder: burnout ≥ 80%, bentonite: blue absorption ≥ 30%, bauxite: Al2O3 ≥ 60%, limestone: CaO ≥ 60%, phenolic resin: burnt carbon residue rate ≥ 50%, pregelatinized starch: viscosity ≥ 700 mPa·s.
[0064] (2) crushing the organic binder, bauxite and limestone to a particle size of ≤5 mm;
[0065] (3) Weighing 20 to 80 parts of crushed organic binder, 5 to 40 parts of bentonite, 2 to 10 parts of bauxite, 2 to 20 parts of limestone, 2 to 20 parts of phenolic resin, and 5 to 30 parts of pregelatinized starch respectively according to weight ratio, mixing them together in sequence, and stirring to mix them evenly;
[0066] (4) The mixture is further dry-ground to make the particle size of the mixture ≤ 0.1 mm to obtain a transitional binder.
[0067] The transitional binder prepared as above can be used to prepare high-strength carbon-containing pellets, solving the problems of poor strength and severe pulverization of carbon-containing pellets during calcination in the prior art.
[0068] A method for preparing high-strength carbon-containing pellets of the present invention specifically comprises the following steps:
[0069] S1, mixing the transitional binder prepared above with iron ore powder and reduced carbon in a certain proportion to obtain a mixture;
[0070] Specifically, firstly, iron ore powder and reduced carbon are selected. The quality indicators of iron ore powder are: total iron content ≥55wt%, S content ≤0.6wt%, P content ≤0.1wt%; the mass proportion of the part with particle size ≤0.074 is greater than 80%. The quality indicators of reduced carbon are: dry basis volatile matter content ≤20wt%, dry basis ash content ≤15wt%, dry basis fixed carbon content ≥70wt%, dry basis S content ≤0.5wt%; the mass proportion of the part with particle size ≤0.074 is greater than 70%.
[0071] Then, the transitional binder is uniformly mixed with the iron ore powder and the reduced carbon in a weight ratio of 2-10:70-80:10-20 to obtain a mixture.
[0072] In a specific embodiment, the iron ore powder includes one or a mixture of magnetite, hematite, limonite, goethite, and vanadium-ferromagnetite; the reducing carbon includes one or a mixture of anthracite, bituminous coal, upgraded coal, lignite, biochar, pyrolytic carbon black, and coke powder.
[0073] S2, adding water to the mixture, stirring and mixing, and then cold pressing to obtain carbon-containing wet pellets;
[0074] Specifically, water is added at 3-10wt% of the mixture, and the mixture is stirred and mixed before cold pressing, wherein the molding pressure is selected from 5 to 100 MPa, and carbon-containing wet pellets are obtained under the molding pressure conditions; the compressive strength of the carbon-containing wet pellets is ≥150N / piece, the 0.5m drop strength is ≥3 times, and the thermal burst temperature is ≥500°C; in a further embodiment, the 0.5m drop strength of the carbon wet pellets is ≥4 times, and the thermal burst temperature is ≥730°C.
[0075] S3, drying the carbon-containing wet pellets in a drying furnace to obtain high-strength carbon-containing pellets, wherein the drying temperature of the drying treatment is 90 to 250° C. and the drying time is 0.5 to 3 hours.
[0076] The main strength indicators of the high-strength carbon-containing pellets prepared above are: the compressive strength of the high-strength carbon-containing pellets is ≥2000N / piece, and the 0.5m drop strength is ≥15 times; the high-temperature compressive strength of the high-strength carbon-containing pellets after calcining at 600°C is ≥1000N / piece, and the 0.5m drop strength is ≥15 times; the high-temperature compressive strength of the high-strength carbon-containing pellets after calcining at 900°C is ≥300N / piece, and the 0.5m drop strength is ≥15 times; the high-temperature compressive strength of the high-strength carbon-containing pellets after calcining at 1200°C is ≥2000N / piece, the 3m drop strength is ≥5 times, and the metallization rate is ≥80%.
[0077] In a further specific embodiment, the compressive strength of the high-strength carbon-containing pellets is ≥2100N / piece, and the 0.5m drop strength is ≥25 times. The high-temperature compressive strength of the high-strength carbon-containing pellets after 600°C roasting is 2500-3000N / piece, and the 0.5m drop strength is ≥50 times. The high-temperature compressive strength of the high-strength carbon-containing pellets after 900°C roasting is ≥600N / piece. The high-temperature compressive strength of the high-strength carbon-containing pellets after 1200°C roasting is ≥4000N / piece, and the 3m drop strength is ≥10 times.
[0078] The transitional binder and preparation method of the present invention and the method for preparing high-strength carbon-containing pellets are further introduced below with reference to specific examples.
[0079] Example 1
[0080] The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0081] (1) Selecting the raw materials of the transitional binder, the composition and quality indicators thereof are as follows: organic binder (using polyvinyl alcohol): burning loss is 88.5%, bentonite: blue absorption is 52.7%, bauxite: Al2O3 content is 68.3%, limestone: CaO content is 73.8%, phenolic resin: burning residual carbon rate is 59.3%, pregelatinized starch (using corn pregelatinized starch): viscosity is 860 mPa·s;
[0082] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0083] (3) Weighing 50 kg of crushed organic binder, 10 kg of bentonite, 5 kg of bauxite, 15 kg of limestone, 10 kg of phenolic resin, and 10 kg of pregelatinized starch respectively, and mixing them together in sequence, and stirring to mix them evenly;
[0084] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0085] (5) Select iron ore powder (magnetite), the quality indicators of magnetite are: total iron content is 63.5%, the mass proportion of the part with a particle size of ≤0.074 mm is 85%, the S content is 0.3%, and the phosphorus content is 0.05%;
[0086] (6) Selecting reduced carbon (using upgraded coal), the quality indicators of upgraded coal are: dry basis volatile matter content is 18.3%, dry basis ash content is 8.7%, dry basis fixed carbon content is 73%, dry basis S content is 0.4%, and the mass proportion of the part with a particle size of ≤0.074 mm is 73.5%;
[0087] (7) The transition binder, magnetite and upgraded coal are mixed in a weight ratio of 8:79:13 to obtain a mixture, water is added according to 5% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 35 MPa. Wet carbon-containing pellets are obtained under the molding pressure conditions. The obtained carbon-containing pellets are dried in a drying furnace at 105° C. for 2 hours to obtain high-strength carbon-containing pellets.
[0088] Comparative Example 1
[0089] The same iron ore powder was used, and the transitional binder was changed to a finely ground bentonite binder. The bentonite binder, magnetite and upgraded coal were mixed uniformly in the same proportion as in Example 1, and water was added according to a mass fraction of 5% of the mixture. After stirring evenly, cold pressing was performed, and the same molding pressure, drying temperature and drying time as in Example 1 were selected to obtain carbon-containing pellets for control.
[0090] The carbon-containing pellets prepared in Example 1 and Comparative Example 1 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0091] Example 2
[0092] 1 The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0093] (1) Selecting the raw materials of the transitional binder, the composition and quality indicators thereof are as follows: organic binder (using acetic acid copolymer): burning loss is 91.7%, bentonite: blue absorption is 63.2%, bauxite: Al2O3 content is 63.1%, limestone: CaO content is 70.5%, phenolic resin: burning residual carbon rate is 63.5%, pregelatinized starch (using cassava pregelatinized starch): viscosity is 930 mPa·s;
[0094] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0095] (3) Weighing 60 kg of crushed organic binder, 15 kg of bentonite, 5 kg of bauxite, 5 kg of limestone, 5 kg of phenolic resin, and 10 kg of pregelatinized starch respectively, and mixing them together in sequence, and stirring to mix them evenly;
[0096] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0097] (5) Select iron ore powder (using vanadium-titanium magnetite), the quality indicators of vanadium-titanium magnetite are: total iron content is 55.7%, the mass proportion of the part with a particle size of ≤0.074 mm is 83%, the S content is 0.35%, and the phosphorus content is 0.06%;
[0098] (6) Selecting reduced carbon (using anthracite), the quality indicators of anthracite are: dry basis volatile matter content is 7.6%, dry basis ash content is 11.7%, dry basis fixed carbon content is 80.7%, dry basis S content is 0.43%, and the mass proportion of the part with a particle size of ≤0.074 mm is 77.8%;
[0099] (7) The transition binder is mixed with vanadium-titanium magnetite and anthracite in a weight ratio of 6:82:12 to obtain a mixture, water is added according to 6% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 53 MPa. Under the molding pressure, wet carbon-containing pellets are obtained. The obtained carbon-containing pellets are dried in a drying furnace at 105° C. for 2 hours to obtain high-strength carbon-containing pellets.
[0100] Comparative Example 2
[0101] The same iron ore powder was used, and the transitional binder was replaced with a finely ground water glass binder. The water glass binder, vanadium-titanium magnetite and anthracite were mixed uniformly in the same proportion as in Example 2. Water was added at a mass fraction of 6% of the mixture, and the mixture was stirred evenly before cold pressing. The same molding pressure, drying temperature and drying time as in Example 2 were selected to obtain carbon-containing pellets for control.
[0102] The carbon-containing pellets prepared in Example 2 and Comparative Example 2 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0103] Example 3
[0104] 1 The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0105] (1) Selecting the raw materials of the transitional binder, the composition and quality indicators thereof are as follows: organic binder (using polyvinyl alcohol): burning loss is 88.5%, bentonite: blue absorption is 48.3%, bauxite: Al2O3 content is 66.8%, limestone: CaO content is 65.3%, phenolic resin: burning residual carbon rate is 58.7%, pregelatinized starch (using wheat pregelatinized starch): viscosity is 1140 mPa·s;
[0106] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0107] (3) Weighing 70 kg of crushed organic binder, 10 kg of bentonite, 2 kg of bauxite, 3 kg of limestone, 5 kg of phenolic resin, and 10 kg of pregelatinized starch respectively, and mixing them together in sequence, and stirring to mix them evenly;
[0108] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0109] (5) Select iron ore powder (hematite), the quality indicators of hematite are: total iron content is 63.8%, the mass proportion of the part with a particle size of ≤0.074 mm is 82%, the S content is 0.42%, and the phosphorus content is 0.05%;
[0110] (6) Selecting reduced carbon (using biochar), the quality indicators of biochar are: dry basis volatile matter content is 13.5%, dry basis ash content is 3.3%, dry basis fixed carbon content is 83.2%, dry basis S content is 0.05%, and the mass proportion of the part with a particle size of ≤0.074 mm is 71.8%;
[0111] (7) The transition binder is mixed with hematite and biochar in a weight ratio of 5:82:13 to obtain a mixture, water is added according to 5.5% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 67 MPa. Wet carbon-containing pellets are obtained under the molding pressure conditions. The obtained carbon-containing pellets are dried in a drying furnace at 105° C. for 2 hours to obtain high-strength carbon-containing pellets.
[0112] Comparative Example 3
[0113] The same iron ore powder was used, and the transitional binder was changed to a syrup binder. The syrup binder, hematite and biochar were mixed uniformly in the same proportion as in Example 3, and water was added according to a mass fraction of 5.5% of the mixture. After stirring evenly, cold pressing was performed, and the same molding pressure, drying temperature and drying time as in Example 3 were selected to obtain carbon-containing pellets for control.
[0114] The carbon-containing pellets prepared in Example 3 and Comparative Example 3 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0115] Example 4
[0116] The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0117] (1) Selecting the raw materials of the transition state binder, the composition and quality indicators thereof are as follows: organic binder (using polyoxymethylene): burning loss is 85.8%, bentonite: blue absorption is 38.5%, bauxite: Al2O3 content is 61.8%, limestone: CaO content is 66.4%, phenolic resin: burning residual carbon rate is 53.5%, pregelatinized starch (using rice pregelatinized starch): viscosity is 1338 mPa·s;
[0118] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0119] (3) Weighing 50 kg of crushed organic binder, 20 kg of bentonite, 5 kg of bauxite, 5 kg of limestone, 5 kg of phenolic resin, and 15 kg of pregelatinized starch respectively, and mixing them together in sequence, and stirring to mix them evenly;
[0120] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0121] (5) Select iron ore powder (magnetite and hematite), mix the magnetite and hematite in a ratio of 8:2, and the quality indicators of the mixed ore are: total iron content is 62.5%, the mass proportion of the part with a particle size of ≤0.074 mm is 87%, the S content is 0.41%, and the phosphorus content is 0.03%;
[0122] (6) Selecting reduced carbon (using blue carbon), the quality indicators of blue carbon are: dry basis volatile matter content is 11.3%, dry basis ash content is 10.3%, dry basis fixed carbon content is 78.4%, dry basis S content is 0.33%, and the mass proportion of the part with a particle size of ≤0.074 mm is 76.3%;
[0123] (7) The transition binder is mixed with hematite and biochar in a weight ratio of 6:81:13 to obtain a mixture, water is added according to 6.5% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 85 MPa. Wet carbon-containing pellets are obtained under the molding pressure conditions. The obtained carbon-containing pellets are dried in a drying furnace at 105° C. for 2 hours to obtain high-strength carbon-containing pellets.
[0124] Comparative Example 4
[0125] The same iron ore powder was used, and the transitional binder was changed to yellow dextrin binder. The yellow dextrin binder, iron ore powder (i.e., mixed ore) and lignite were mixed uniformly in the same proportion as in Example 4. Water was added according to a mass fraction of 6.5% of the mixture. After stirring evenly, cold pressing was performed. The same molding pressure, drying temperature and drying time as in Example 4 were selected to obtain carbon-containing pellets for control.
[0126] The carbon-containing pellets prepared in Example 4 and Comparative Example 4 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0127] Example 5
[0128] The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0129] (1) Select the raw materials of the transition state binder, and its composition and quality indicators are as follows: organic binder (using paraffin wax): burning loss is 81.1%, bentonite: blue absorption is 37.6%, bauxite: Al2O3 content is 62.5%, limestone: CaO content is 67.3%, phenolic resin: burning residual carbon rate is 55.7%, pregelatinized starch (using potato pregelatinized starch): viscosity is 1138 mPa·s;
[0130] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0131] (3) Weighing 20 kg of crushed organic binder, 30 kg of bentonite, 10 kg of bauxite, 10 kg of limestone, 10 kg of phenolic resin, and 20 kg of pregelatinized starch respectively, mixing them together in sequence, and stirring to mix them evenly;
[0132] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0133] (5) Select iron ore powder (magnetite and hematite), mix the magnetite and hematite in a ratio of 3:7, and the quality indicators of the mixed ore are: total iron content is 61.3%, the mass proportion of the part with a particle size of ≤0.074 mm is 73%, the S content is 0.42%, and the phosphorus content is 0.03%;
[0134] (6) Selecting reduced carbon (using blue carbon), the quality indicators of blue carbon are: dry basis volatile matter content is 12.5%, dry basis ash content is 11.1%, dry basis fixed carbon content is 76.4%, dry basis S content is 0.35%, and the mass proportion of the part with a particle size of ≤0.074 mm is 78.5%;
[0135] (7) The transition binder is mixed with hematite and biochar in a weight ratio of 6:82:12 to obtain a mixture, water is added according to 7.4% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 80 MPa. Wet carbon-containing pellets are obtained under the molding pressure conditions. The obtained carbon-containing pellets are dried in a drying furnace at 150° C. for 1 hour to obtain high-strength carbon-containing pellets.
[0136] Comparative Example 5
[0137] The same iron ore powder was used, and the transitional binder was changed to a water glass binder. The water glass binder, iron ore powder (i.e., mixed ore) and lignite were mixed uniformly in the same proportion as in Example 5. Water was added according to a mass fraction of 7.4% of the mixture. After stirring evenly, cold pressing was performed. The same molding pressure, drying temperature and drying time as in Example 5 were selected to obtain carbon-containing pellets for control.
[0138] The carbon-containing pellets prepared in Example 5 and Comparative Example 5 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0139] Example 6
[0140] The preparation method of the transitional binder and high-strength carbon-containing pellets in this embodiment is as follows:
[0141] (1) Selecting the raw materials of the transition state binder, the composition and quality indicators thereof are as follows: organic binder (using polyoxymethylene): burning loss is 85.8%, bentonite: blue absorption is 37.6%, bauxite: Al2O3 content is 63.8%, limestone: CaO content is 67.9%, phenolic resin: burning residual carbon rate is 55.2%, pregelatinized starch (using rice pregelatinized starch): viscosity is 1338 mPa·s;
[0142] (2) crushing the organic binder, bauxite and limestone in the raw materials of the transitional binder to a particle size of ≤5 mm;
[0143] (3) Weighing 80 kg of crushed organic binder, 5 kg of bentonite, 2 kg of bauxite, 2 kg of limestone, 2 kg of phenolic resin, and 9 kg of pregelatinized starch respectively, and mixing them together in sequence, and stirring to mix them evenly;
[0144] (4) The mixture is further dry-ground to a particle size of ≤0.1 mm, which is a transitional binder;
[0145] (5) iron ore powder (magnetite and hematite) was selected, and the magnetite and hematite were mixed in a ratio of 5:5. The quality indicators of the mixed ore were as follows: the total iron content was 61.7%, the mass proportion of the part with a particle size of ≤0.074 mm was 83%, the S content was 0.45%, and the phosphorus content was 0.02%;
[0146] (6) Selecting reduced carbon (using blue carbon), the quality indicators of blue carbon are: dry basis volatile matter content is 10.1%, dry basis ash content is 10.2%, dry basis fixed carbon content is 79.7%, dry basis S content is 0.35%, and the mass proportion of the part with a particle size of ≤0.074 mm is 77.1%;
[0147] (7) The transition binder is mixed with hematite and biochar in a weight ratio of 10:80:10 to obtain a mixture, water is added according to 7.8% of the mass fraction of the mixture, and the mixture is stirred and mixed before cold pressing. The molding pressure is 70 MPa. Wet carbon-containing pellets are obtained under the molding pressure conditions. The obtained carbon-containing pellets are dried in a drying furnace at 180° C. for 1 hour to obtain high-strength carbon-containing pellets.
[0148] Comparative Example 6
[0149] The same iron ore powder was used, and the transitional binder was changed to bentonite binder. The bentonite binder, iron ore powder (i.e., mixed ore) and lignite were mixed uniformly in the same ratio as in Example 6. Water was added according to a mass fraction of 7.8% of the mixture. After stirring evenly, cold pressing was performed. The same molding pressure, drying temperature and drying time as in Example 5 were selected to obtain carbon-containing pellets for control.
[0150] The carbon-containing pellets prepared in Example 6 and Comparative Example 6 were calcined in a high-temperature muffle furnace under a protective atmosphere. The calcination temperatures were 600°C, 900°C and 1200°C, respectively, and the calcination time was 30 min. The high-temperature compressive strength and 0.5 m drop strength of the calcined pellets were measured using a compressive strength tester and a drop strength tester. The total iron content and metallic iron content of the calcined pellets were determined by chemical analysis methods. The metallization rate of the reduced pellets was calculated based on the total iron content and the metallic iron content. The test results are shown in Table 1.
[0151] Table 1 Comparison of compressive strength, drop strength and metallization rate of carbon-containing pellets
[0152]
[0153] Compared with the comparative example, the transitional binder prepared in the embodiment of the present invention has the effect of direct bonding of cold and hot strength, can improve the cold and hot strength of carbon-containing pellets, and improve the metallurgical properties of carbon-containing pellets. As shown in Table 1, the thermal burst temperature of the wet pellets obtained in Examples 1-6 of the present invention is ≥500°C, and the thermal burst temperature of the wet pellets obtained in most embodiments (except for Example 5) is between 730 and 830°C. The compressive strength of the high-strength carbon-containing pellets is ≥2000N / piece, and the 0.5m drop strength is ≥15 times. The compressive strength of the high-strength carbon-containing pellets obtained in most embodiments (except for Example 5) is between 2100 and 2900N / piece, and the 0.5m drop strength is between 25 and 45 times. The compressive strength of the high-strength carbon-containing pellets calcined at 600°C is ≥1000N / piece, and the 0.5m drop strength is 15 times; in most embodiments (except for the embodiments of Example 5), the compressive strength of the high-strength carbon-containing pellets calcined at 600°C is between 2500 and 3000N / piece, and the 0.5m drop strength is between 55 and 85 times. The compressive strength of the high-strength carbon-containing pellets calcined at 900°C is ≥300N / piece, and the 0.5m drop strength is ≥15 times; in most embodiments (except for the embodiments of Example 5), the compressive strength of the high-strength carbon-containing pellets calcined at 900°C is between 600 and 950N / piece, and the 0.5m drop strength is between 17 and 40 times. The compressive strength of the high-strength carbon-containing pellets after 1200 calcination is ≥4000N / piece, the 3m drop strength is ≥10 times, and the metallization rate is ≥80%; in most embodiments (except embodiment 5), the compressive strength of the high-strength carbon-containing pellets after 1200 calcination is between 4300 and 5500N / piece, the 3m drop strength is between 15 and 25 times, and the metallization rate is ≥83%.
[0154] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A transitional binder, characterized in that: The raw materials include the following components by weight:
2. The transitional binder according to claim 1, characterized in that: The burnout of the organic binder is ≥80%; and / or The bentonite has an absorption capacity of ≥30%; and / or The content of Al2O3 in the bauxite is ≥ 60wt%; and / or The content of CaO in the limestone is ≥ 60%; and / or The phenolic resin has a residual carbon rate of ≥50%; and / or The viscosity of the pregelatinized starch is ≥700 mPa·s.
3. The transitional binder according to claim 1, characterized in that: The organic binder is one or more of paraffin beeswax, polyoxymethylene, polyvinyl alcohol, and acetic acid copolymer; and / or The pregelatinized starch is one or more of corn pregelatinized starch, wheat pregelatinized starch, potato pregelatinized starch, cassava pregelatinized starch, and rice pregelatinized starch.
4. The transitional binder according to claim 1, characterized in that: The particle sizes of the organic binder, bauxite and limestone are all ≤5mm.
5. A method for preparing a transitional binder according to any one of claims 1 to 4, characterized in that: An organic binder, bentonite, bauxite, limestone, phenolic resin and pregelatinized starch are mixed in proportion and stirred evenly to obtain a mixture, and the mixture is ground into a particle size of ≤0.1 mm by dry grinding to obtain a transitional binder.
6. A method for preparing high-strength carbon-containing pellets, characterized in that: The following steps are involved: S1, mixing the transitional binder according to any one of claims 1 to 4 with iron ore powder and reduced carbon in a certain proportion to obtain a mixture; S2, adding water to the mixture, stirring and mixing, and then cold pressing to obtain carbon-containing wet pellets; S3, drying the carbon-containing wet pellets to obtain high-strength carbon-containing pellets.
7. The method for preparing high-strength carbon-containing pellets according to claim 6, characterized in that: In step S1: The iron ore powder has a total iron content of ≥55wt%, an S content of ≤0.6wt%, and a P content of ≤0.1wt%; and / or In the iron ore powder, the mass proportion of the part with a particle size of ≤0.074 is greater than 80%; and / or The reduced carbon has a dry basis volatile matter content of ≤20wt%, a dry basis ash content of ≤15wt%, a dry basis fixed carbon content of ≥70wt%, and a dry basis S content of ≤0.5wt%; and / or In the reduced carbon, the mass proportion of the part with a particle size of ≤0.074 is greater than 70%; and / or The weight ratio of the transitional binder to the iron ore powder and the reduced carbon is 2-10:70-80:10-20.
8. The method for preparing high-strength carbon-containing pellets according to claim 6, characterized in that: In step S1: The iron ore powder includes one or a mixture of magnetite, hematite, limonite, goethite, and vanadium-iron magnetite; and / or The reducing carbon includes one or a mixture of anthracite, bituminous coal, upgraded coal, semi-coke, biomass charcoal, pyrolytic carbon black, and coke powder.
9. The method for preparing high-strength carbon-containing pellets according to claim 6, characterized in that: In step S2: The amount of water added is 3-10 wt% of the mixture; and / or The cold press forming pressure is 5 to 100 MPa; and / or The carbon-containing wet pellets have a compressive strength of ≥150N / piece, a 0.5m drop strength of ≥3 times, and a thermal burst temperature of ≥500°C.
10. The method for preparing high-strength carbon-containing pellets according to claim 9, characterized in that: The carbon-containing wet pellets have a 0.5 m drop strength of ≥4 times, and a thermal burst temperature of ≥730°C.
11. The method for preparing high-strength carbon-containing pellets according to claim 6, characterized in that: In step S3: The high-strength carbon-containing pellets have a compressive strength of ≥2000N / piece and a 0.5m drop strength of ≥15 times; and / or The high-strength carbon-containing pellets calcined at 600°C have a high-temperature compressive strength of ≥1000N / piece and a 0.5m drop strength of ≥15 times; and / or The high-strength carbon-containing pellets calcined at 900°C have a high-temperature compressive strength of ≥300N / piece and a 0.5m drop strength of ≥15 times; and / or The high-strength carbon-containing pellets calcined at 1200°C have a high-temperature compressive strength of ≥2000N / piece, a 3m drop strength of ≥5 times, and a metallization rate of ≥80%.
12. The method for preparing high-strength carbon-containing pellets according to claim 11, characterized in that: In step S3: The high-strength carbon-containing pellets have a compressive strength of ≥2100N / piece and a 0.5m drop strength of ≥25 times; and / or The high-strength carbon-containing pellets calcined at 600°C have a high-temperature compressive strength of 2500-3000N / piece and a 0.5m drop strength of ≥50 times; and / or The high-temperature compressive strength of the high-strength carbon-containing pellets after calcination at 900°C is ≥600N / piece; and / or The high-strength carbon-containing pellets calcined at 1200°C have a high-temperature compressive strength of ≥4000N / piece and a 3m drop strength of ≥10 times.