Steel for cryogenic container and manufacturing method thereof
By optimizing the chemical composition and heat treatment process of the steel plate, forming steel for deep-cooled containers suitable for -196℃ environment, the problem that the existing technology cannot effectively manufacture steel for liquefied natural gas storage tanks and containers has been solved, and high and low temperature toughness and Low cost material preparation.
Patent Information
- Application Number
- CN202310623963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot effectively manufacture steel for liquefied natural gas (LNG) storage tanks and containers suitable for low temperature environments of -196°C, and the manufacturing cost of common materials is relatively high.
By optimizing the chemical composition and heat treatment process of the steel plate, a steel for deep-cooled container was designed, with components including C, Si, Mn, Ni and other elements, satisfying C+4Mn+2Ni≥12.5%, and smelting, rolling, and once The process of quenching, secondary quenching and tempering forms 90-95% tempered martensite and 5-10% reverse austenite microstructure.
The steel plate has high and low temperature toughness at -196°C, the yield strength is greater than 390MPa, the tensile strength is 530-710MPa, the elongation is more than 20%, the impact absorption energy reaches more than 200J, and the manufacturing cost of the material is reduced.
Smart Images

Figure CN119061325A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to steel for containers, and in particular to steel for cryogenic containers and a manufacturing method thereof. Background Art
[0002] Natural gas is a cleaner primary energy source than oil, coal, etc. It is an important form of energy for reducing carbon emissions worldwide. Therefore, the demand for natural gas has increased rapidly in recent years. At -163°C, natural gas is liquefied and its volume is reduced by 600 times, which is very conducive to transoceanic transportation and storage. However, due to the extremely low temperature, the storage and transportation of liquefied natural gas must use special cryogenic materials, such as 9% nickel steel, stainless steel, aluminum alloy, etc. These materials contain a lot of alloy elements such as nickel, resulting in high manufacturing costs.
[0003] For example, Chinese patent CN103509999A discloses a method for manufacturing high nickel steel for cryogenic storage tanks, wherein the weight percentage of the components is: C: 0.01-0.10%, Si: 0.10-0.35%, Mn: 0.30-0.80%, Ni: 4.50-6.00%, S≤0.005%, P≤0.008%, A1s: 0.015-0.050%, and the heat treatment process is quenching after heat preservation at 800-850℃, air cooling after heat preservation and tempering at 550-600℃, to obtain tempered bainite structure, and ensure the strength and low temperature toughness of the steel plate. However, the high nickel steel plate manufactured by the invention is only suitable for the requirement of low temperature toughness at -120℃.
[0004] Chinese patent CN104988420A discloses a V-containing 5Ni steel and a manufacturing method thereof, wherein the chemical composition by weight is: C: 0.045-0.075%, Si: 0.15-0.25%, Mn: 0.50-0.80%, S: ≤0.005%, P: ≤0.008%, Ni: 4.75-5.25%, V: 0.03%-0.05%, A1t: 0.020-0.050%. The steel is made of medium and thick plates and adopts a heat treatment process of offline quenching (800-850°C) + tempering (580-640°C), which can meet the impact energy requirement of -130°C.
[0005] Chinese patent CN104388838A discloses a 5Ni steel plate for ultra-low temperature pressure vessels and a production method thereof, which includes smelting, continuous casting, heating, rolling, cooling and heat treatment processes; the weight percentage of the chemical composition of the steel plate is: C0.07%-0.10%, Si0.15%-0.30%, Mn0.70%-0.80%, P≤0.008%, S≤0.003%, Ni4.90%-5.25%, Alt0.020%-0.050%, As≤0.012%, Sn≤0.015%, Sb≤0.003%, and the balance is Fe and trace inevitable impurities. The method adopts the design of low carbon equivalent components and the production process of controlled rolling and controlled cooling + heat treatment to produce 8-50mm thick continuous casting type 5%Ni steel plates that meet the requirements of low temperature pressure vessels. The heat treatment process: after cooling, the steel plate is subjected to two quenching and tempering treatments; the two quenching temperatures are 840℃±10℃ and 750℃±10℃ respectively, and then water cooling: tempering at 600±10℃ and then air cooling. The steel plate can achieve the requirements of -125℃ low temperature impact toughness.
[0006] Chinese patent CN103103441A discloses a steel for pressure vessels with high toughness at -140°C, whose components and contents are: C≤0.05%, Si≤0.05%, Mn: 0.50-1.00%, P≤0.006%, S≤0.003%, Alt: 0.015-0.050%, Ni: 4.50-5.30%, Nb: 0.02-0.05%, Ti: 0.008-0.025%, N≤0.004%, and further contains one or more of Cr≤0.50%, Mo≤0.50%, Cu≤0.30%, and Ca≤0.005%. The process is: smelting and continuous casting into billets; heating the billets; first-stage rough rolling; second-stage rough rolling after the first temperature treatment; finish rolling after the second temperature treatment; and heat treatment according to the thickness of the steel plate. When the thickness of the steel plate is greater than 40-60mm, the heat treatment is carried out by secondary quenching + tempering, specifically: the first quenching is 800-900℃, the second quenching is 750-850℃, and the tempering is 600-680℃. The KV2 of this pressure vessel steel is not less than 100J at -140℃, the transverse crack thickness rate CTR≤3%, the transverse crack length rate CLR≤10%, the transverse crack sensitivity rate CSR≤1.5%, the Ni content is low, and the welding performance is excellent. However, its low-temperature impact toughness only meets the requirements of -140℃, and cannot be used for LNG storage tanks and containers required at -196℃.
[0007] Chinese patent CN104988404A discloses a nickel-containing steel plate for low temperature of -196°C, whose composition is C≤0.04, Si≤0.05, Mn: 1.60-2.50, P≤0.005, S≤0.003, Alt: 0.015-0.050, Ni: 6.00-8.00, Cu: 0.35-0.50, Cr: 0.55-1.00, N≤0.004, and also contains one or more of Mo≤0.35, Nb≤0.05, Ti≤0.025, and Ca≤0.005. The requirements of low temperature impact toughness at -196°C are achieved by adopting a heat treatment method of 840-890°C primary quenching, 670-830°C secondary quenching and 580-650°C tempering. However, the nickel content of the invention is 6.0-8.0, and alloy elements such as Cr, Mo, and Cu also need to be added, so the alloy cost of the material is relatively high. Summary of the invention
[0008] The object of the present invention is to provide a steel for cryogenic containers and a method for manufacturing the same. The steel plate has a yield strength greater than 390 MPa, a tensile strength of 530 to 710 MPa, and an elongation of more than 20%. More importantly, the steel plate has an impact absorption energy of more than 200 J at -196°C. The steel plate having such toughness can be used in a cryogenic environment as low as -196°C, for the manufacture of liquefied natural gas (LNG) storage tanks and pressure vessels, and the cost is significantly lower than conventional LNG materials such as 9Ni steel and 304L stainless steel.
[0009] To achieve the above object, the technical solution of the present invention is:
[0010] A steel for cryogenic containers, the components of which are as follows by weight: C 0.03-0.08%, Si 0.10-0.25%, Mn 0.3-0.8%, S≤0.005%, P≤0.006%, Ni 4.6-5.5%, the balance comprising Fe and other unavoidable impurities; and, at the same time, the following conditions must be met: C+4Mn+2Ni≥12.5%.
[0011] Furthermore, the balance is Fe and other inevitable impurities.
[0012] Preferably, the composition of the steel for cryogenic containers of the present invention further includes Mo≤0.10wt%, and / or Al≤0.05wt%.
[0013] The microstructure of the steel for cryogenic containers of the present invention is 90-95% tempered martensite + 5-10% reversed austenite.
[0014] The steel for cryogenic containers of the present invention has a yield strength greater than 390 MPa, a tensile strength of 530-710 MPa, an elongation of more than 20%, and an impact absorption energy of more than 200 J at -196°C.
[0015] In the composition design of the steel for cryogenic containers of the present invention:
[0016] Carbon: Carbon is not good for low temperature toughness, but the interstitial solid solution of carbon atoms in the BCC lattice greatly improves the matrix strength. To meet the requirements of comprehensive strength and toughness, a small amount of carbon needs to be added to the steel to ensure it. The control range of the carbon content in the present invention is 0.03-0.08%.
[0017] Silicon: Silicon is a ferrite stabilizing element. Adding it to steel can hinder the formation of carbides, reduce the source of low-temperature cleavage cracking in steel, and help improve low-temperature toughness. However, too high a silicon content increases the brittleness of the steel. The control range of the silicon content in the present invention is 0.10-0.25%.
[0018] Manganese: Manganese plays a role in solid solution strengthening and can improve the strength of the steel plate. In addition, manganese can effectively improve the hardenability of the steel plate, ensuring that the designed structure and target performance are obtained when the thick steel plate is quenched, but high manganese content is prone to segregation. The Mn content of the present invention is in the range of 0.3-0.8%.
[0019] Sulfur: Sulfur is a harmful residual element. It can form MnS inclusions when combined with manganese. It deforms and elongates during rolling, which is not conducive to the uniformity of mechanical properties, especially low-temperature toughness. The sulfur content is required to be less than 0.005%.
[0020] Phosphorus: Phosphorus is also a harmful residual element, which has a great influence on low temperature toughness and is easily segregated on austenite grain boundaries. Therefore, the phosphorus content of the present invention is less than 0.006%.
[0021] Nickel: Nickel is the most important alloy element for improving low-temperature toughness. It can effectively improve the low-temperature cleavage strength of the matrix and reduce the tough-to-brittle transition temperature. In addition, nickel is distributed and enriched in the reversed austenite during heat treatment, which can further improve low-temperature toughness. However, nickel is also an expensive alloy, and adding too much increases the cost. The Ni content of the present invention is in the range of 4.6-5.5%.
[0022] Molybdenum: Molybdenum can greatly improve hardenability. A small amount of addition is beneficial for thick steel plates to achieve target performance and has little effect on low-temperature toughness. Molybdenum alloys are expensive, and the molybdenum content of the present invention is controlled to not exceed 0.10%.
[0023] Aluminum: It is an additive element. Aluminum is a deoxidizer in converter steelmaking. Residual aluminum combines with nitrogen in steel to form AlN particles. The dissolution temperature is very high, which can play a role in pinning grain boundaries and refining grains. In the present invention, aluminum can be added in an amount not exceeding 0.05%.
[0024] The composition design of the present invention must also simultaneously satisfy C+4Mn+2Ni≥12.5%.
[0025] C, Mn, and Ni are all austenite-forming elements, which are easily enriched in a small amount of austenite formed during phase transformation to increase its supercooling stability, and are retained as a "tough phase" to low temperatures, ultimately achieving the effect of material toughening. In order to ensure that these reversed austenites do not decompose during cooling, C, Mn, and Ni are added at the same time, and the combination must meet C+4Mn+2Ni≥12.5%, thereby exerting a combined effect of increasing the stability of austenite.
[0026] The method for manufacturing steel for cryogenic containers of the present invention comprises the following steps:
[0027] 1) Smelting and casting
[0028] Smelting, refining outside the furnace and casting into slabs according to the above ingredients;
[0029] 2) Rolling
[0030] The slab is heated to 1000-1200℃, dephosphorized with high-pressure water, the compression ratio is controlled to be ≥3 during rolling, and the final rolling temperature is 850-930℃;
[0031] 3) Primary quenching, heating to 780-850°C, keeping warm for 0.5-3 hours to make the internal temperature of the steel plate fully uniform, and water cooling to room temperature after the end of the insulation;
[0032] 4) Secondary quenching: reheat at 650-730°C, keep warm for 0.5-1.5 hours, then water cool to room temperature;
[0033] 5) Tempering treatment, tempering temperature 550 ~ 650 ℃, keep warm for 1 to 4 hours.
[0034] In the method for manufacturing steel for cryogenic containers of the present invention:
[0035] The steel billet is heated to 1000-1200℃ to homogenize the austenite structure and fully dissolve the carbides in the steel. At the same time, the lower limit of the heating temperature is controlled to take into account the temperature drop of the slab during rolling and ensure that the rolling is completed at the specified temperature. High-pressure water dephosphorization can remove the iron oxide scale generated during heating.
[0036] In order to fully deform the steel plate during rolling, the compression ratio needs to be controlled to be ≥3, and the final rolling temperature is 850-930℃, which is conducive to obtaining uniform and fine austenite grains.
[0037] The rolled steel plate needs to be heat treated to further adjust the performance, and the heat treatment is carried out by the process of primary quenching, secondary quenching and tempering. The rolled steel plate is first quenched once, heated to 780-850℃, and kept warm for 0.5-3 hours to make the internal temperature of the steel plate fully consistent. After the insulation, it is water-cooled to room temperature; then the steel plate is subjected to secondary quenching heat treatment, heated again at 650-730℃, kept warm for 0.5-1.5 hours and then cooled to room temperature; then the steel plate is tempered to adjust the final performance, the tempering temperature is 550-650℃, and kept warm for 1-4 hours to reduce quenching stress and form a stable organization.
[0038] The key components of the steel for cryogenic containers described in the present invention are C, Mn and Ni elements, all of which are austenite forming elements. In order to ensure a certain austenite forming ability, the content of the three elements must meet C+4Mn+2Ni≥12.5%. Such a composition forms a martensite structure with a fine lath substructure after rapid cooling in the first quenching. Since the temperature of the secondary quenching is 650-730°C in the two-phase region, part of the structure will be transformed into austenite. During the heating and heat preservation process, the three austenite forming elements C, Mn and Ni will be more distributed to the newly generated austenite. During the secondary quenching cooling process, this austenite has higher stability and is not easy to decompose and transform, so it is retained. The final tempering heat treatment further distributes C, Mn and Ni to the austenite with high stability, thereby increasing its stability. Finally, a microstructure of tempered martensite + a small amount of reversed austenite is formed, which is very beneficial to improve low-temperature toughness. Tempered martensite has a fine lath substructure with large orientation difference between laths, which can increase the crack propagation resistance and improve low-temperature toughness. Reversed austenite has a oriented cubic (FCC) crystal structure and is dispersed in the matrix structure. As a tough phase, it also hinders the linear propagation of cracks and promotes the passivation of crack tips, which has the effect of significantly improving low-temperature toughness. Finally, the steel plate of the present invention can achieve excellent low-temperature toughness at -196°C without high nickel content.
[0039] Compared with the prior art, the beneficial effects of the present invention are:
[0040] The toughness of steel is closely related to the alloy elements and microstructures contained therein. The present invention provides a basic guarantee for the low-temperature cleavage strength of the matrix structure by adding a reasonable level of Ni and other alloy elements. In addition, this component forms tempered martensite under the quenching and tempering heat treatment process. The structure contains fine sub-structure units, which can effectively reduce dislocation pile-up stress, reduce internal stress concentration of the structure, and play a role in improving low-temperature toughness.
[0041] Another measure adopted by the present invention is to add a secondary quenching heat treatment process to the primary quenching and tempering. By heating the steel plate to the two-phase temperature range where part of austenite is formed, austenite-forming elements such as C, Mn, and Ni are partitioned and enriched in these reversed austenites at high temperatures during a certain holding time, which greatly increases the stability of the reversed austenite. The reversed austenite is retained without transformation during the subsequent quenching and cooling, and the final steel plate structure contains 5% to 10% of reversed austenite. These reversed austenites have a face-centered cubic (FCC) crystal structure and have the advantage of not undergoing a tough-to-brittle transition as the temperature decreases. They are dispersed in the tempered martensite matrix, which can hinder the continued expansion of small cracks, force them to turn and passivate, and increase the energy required for the expansion of cleavage cracks, thereby greatly improving the low-temperature toughness of the steel plate, and finally achieving good low-temperature toughness at -196°C.
[0042] Compared with the prior art, the composition design of the present invention is easy to implement, and the alloying treatment not only effectively strengthens the steel, but also achieves high toughness at -196°C. The present invention does not add alloying element V like Chinese patent CN104988420A, and has a lower Ni content than 6-8% in Chinese patent CN104988404A, and even less than 9% Ni content in conventional 9Ni steel, thereby having a lower manufacturing cost.
[0043] The present invention is different from the heat treatment process of only one quenching and tempering adopted by Chinese patents CN103509999A and CN104988420A, and is also lower than the temperature of 750-850℃ secondary quenching in Chinese patents CN104388838A and CN103103441A, thereby obtaining the optimal ratio of reversed austenite, and indirectly regulating the position and amount of precipitation of these reversed austenites, increasing their supercooling stability, and achieving low-temperature toughness at a lower temperature than these patents. These patents can only be applied to the storage and transportation of low-temperature media such as LEG and LPG, while the present invention can be further used for the storage and transportation of LNG.
[0044] After the above composition and production process, the steel plate of the present invention has a yield strength greater than 390MPa, a tensile strength of 530-710MPa, and an elongation of more than 20%. More importantly, the impact absorption energy of the steel plate at -196°C reaches more than 200J. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a metallographic structure photograph of Example 1 of the present invention;
[0046] Figure 2 This is the EBSD image of Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The present invention will be further described below in conjunction with the embodiments and drawings.
[0048] The chemical composition of the embodiment of the present invention is shown in Table 1, and the balance is Fe and other inevitable impurities. The process parameters of the embodiment are shown in Table 2, and the mechanical properties and reversed austenite content are shown in Table 3.
[0049] The process route of the embodiment of the present invention is: smelting → refining outside the furnace → ingot casting → slab heating → rolling → primary quenching → secondary quenching → tempering → inspection.
[0050] As can be seen from Table 3, the yield strength of the steel plates in the examples all exceeds 390 MPa, the tensile strength is between 530 and 710 MPa, the elongation is all over 20%, and the actual level reaches over 25%, which shows excellent strength and plasticity. In addition, the impact absorption energy at -196°C in Table 3 is all over 200 J.
[0051] See also Figure 1 , which shows the metallographic structure photograph of Example 1 of the present invention, which is mainly a fine tempered martensite structure.
[0052] After heat treatment, the typical microstructure of the embodiment is 90-95% tempered martensite + 5-10% reversed austenite.
[0053] Figure 2 The EBSD image of Example 1 of the present invention also shows a fine lath structure. In addition, the red color in the figure represents the reversed austenite of the face-centered cubic (FCC) structure, which is dispersed at the grain boundaries or between the laths and plays a toughening role.
[0054] In summary, the present invention uses a simple alloying method and adds a small amount of Ni element to the steel, and adopts a heat treatment method of double quenching and tempering to produce a steel plate with good deep low temperature toughness, and the production process is simple and feasible. The product of the present invention can be used for liquefied natural gas LNG storage tanks and containers, and has obvious cost advantages compared with existing materials.
[0055]
[0056]
[0057]
Claims
1. A steel for cryogenic containers, the composition weight percentage of which is: C 0.03~0.08%; Si 0.10~0.25%; Mn 0.3~0.8%; S≤0.005%; P≤0.006%; Ni 4.6~5.5%; The balance includes Fe and other unavoidable impurities; and at the same time must meet the following requirements: C+4Mn+2Ni≥12.5%.
2. The steel for cryogenic containers according to claim 1, It is characterized in that The balance is Fe and other inevitable impurities.
3. The steel for cryogenic containers according to claim 1 or 2, It is characterized in that It also contains Mo≤0.10wt%, and / or Al≤0.05wt%.
4. The steel for cryogenic containers according to claim 1, 2 or 3, It is characterized in that The microstructure of the steel for cryogenic containers is 90-95% tempered martensite + 5-10% reversed austenite.
5. The steel for cryogenic containers according to claim 1, 2, 3 or 4, It is characterized in that The yield strength of the steel for cryogenic containers is greater than 390 MPa, the tensile strength is 530-710 MPa, the elongation is more than 20%, and the impact absorption energy at -196°C reaches more than 200 J.
6. The method for producing a steel for a cryogenic container according to any one of claims 1 to 5, Its characteristics are: The steps include: 1) Smelting and casting Smelting, refining outside the furnace and casting into slabs according to the components of claim 1, 2 or 3; 2) Rolling The slab is heated to 1000-1200℃, dephosphorized with high-pressure water, the compression ratio is controlled to be ≥3 during rolling, and the final rolling temperature is 850-930℃; 3) Primary quenching, heating to 780-850°C, keeping warm for 0.5-3 hours to make the internal temperature of the steel plate fully uniform, and water cooling to room temperature after the end of the insulation; 4) Secondary quenching: reheat at 650-730°C, keep warm for 0.5-1.5 hours, then water cool to room temperature; 5) Tempering treatment, tempering temperature 550 ~ 650 ℃, keep warm for 1 to 4 hours.
Citation Information
Patent Citations
High-tenacity -130 DEG C low-temperature steel and manufacturing method thereof
CN102330031A
5Ni steel plate for ultralow temperature pressure vessel and production method of 5Ni steel plate
CN104388838A
Easy-to-weld container plate with thickness ranging from 40 millimeters to 60 millimeters and excellent center low-temperature toughness, and making method thereof
CN110184531A
Nickel-containing steel sheet for low temperature excellent in tensile strength and toughness and manufacturing method therefor
JP2017160512A