Method for improving low-temperature toughness of core part of large-thickness SA516Gr.70 steel plate
By optimizing chemical composition and preparation process, the problem of low-temperature impact toughness of the core of the large-thick SA516Gr.70 steel plate is solved. By refining the structure and improving element uniformity, the low-temperature impact performance of the steel plate is improved, meeting the market's high-end Technical requirements of equipment.
Patent Information
- Application Number
- CN202411186788.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The low-temperature impact toughness of the core of the large-thick SA516Gr.70 steel plate is unstable, mainly due to the thickness, which leads to serious segregation of elements and large tissues, which affects its low-temperature impact performance.
By optimizing chemical composition and preparation processes, including slab heating, two-stage rolling and normalizing (fast cooling) + tempering heat treatment, the furnace temperature, heat equalization time and deformation amount are controlled, the tissue structure is refined, and element uniformity is improved. Tissue uniformity.
The low-temperature impact toughness of the core of the high-thickness SA516Gr.70 steel plate is significantly improved, meeting the requirements of ASME SA516/SA516M-2023 standards, ensuring the stable performance of the steel plate in extreme environments.
Smart Images

Figure CN119061327A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting, and in particular relates to a method for improving the low-temperature toughness of the core of a thick SA516Gr.70 steel plate. Background Art
[0002] SA516 series steel plates are carbon steel plates for medium and low temperature pressure vessels that comply with ASME standards. They are widely used in the fields of petroleum, chemical industry, nuclear power plants, boilers, etc. due to their excellent low temperature impact toughness, good welding performance and fatigue resistance, and high purity. With the extreme service environment of low temperature pressure vessels and the high-end and large-scale equipment, the market has more diverse and stringent requirements on the physical properties and chemical composition of SA516Gr.70 low alloy steel for heads and cylinders, especially the low temperature impact toughness of the core of thick steel plates. Therefore, higher requirements are put forward for element control and microstructure performance regulation in the production process of thick steel plates. However, due to the thick thickness of SA516Gr.70 steel plates, the alloy element segregation in the core is serious, and the deformation of the core of the steel plate is small during rolling. The cooling rate of the core is slow during the cooling process after heat treatment, which can easily lead to coarse microstructure and uneven element distribution in the core of the steel plate, thereby reducing the low temperature impact toughness of the core of the steel plate. Aiming at the problem of low-temperature impact instability in the core of thick SA516Gr.70 steel plates, in order to meet market demand, the present invention provides a method for improving the low-temperature toughness of the core of thick SA516Gr.70 steel plates, which has important market promotion value. Summary of the invention
[0003] The purpose of the present invention is to improve the low-temperature impact stability of the core of thick SA516Gr.70 steel plates by improving the uniformity of element distribution and the deformation of the core of the steel plates and refining the structure, so as to meet the market technical needs for steel plates for heads and cylinders of large-scale equipment. The improvement of the low-temperature impact stability of the core of thick SA516Gr.70 steel plates can be achieved from the perspective of composition design and preparation process.
[0004] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: in terms of component design, the chemical composition of the steel plate is as follows: C: 0.12% to 0.16%, Si: 0.15% to 0.25%, Mn: 1.40% to 1.50%, P≤0.010%, S≤0.003%, Alt: 0.020% to 0.050%, Nb: 0.015% to 0.02%, V: 0.025% to 0.030%, Ni: 0.30% to 0.40%, Cu: 0.20% to 0.30%, and the others are Fe and essential residual elements.
[0005] The present invention provides a method for improving the low-temperature toughness of the core of a thick SA516Gr.70 steel plate, the method comprising the following steps:
[0006] Slab heating: heating furnace hearth temperature ≤ 1250℃, soaking temperature 1180~1220℃, furnace time ≥ 10h, soaking time 40~60min;
[0007] Rolling: The rolling process is divided into two stages. The starting rolling temperature of stage I is ≥1080℃, the final rolling temperature is ≥980℃, the reduction rate of the last three passes after widening is ≥17%, and the thickness of the intermediate billet is more than twice the thickness of the finished plate; the starting rolling temperature of stage II is ≤880℃, the final rolling temperature is 750~820℃, and the water cooling is rapid after rolling, and the red-returning temperature is 680~720℃;
[0008] Heat treatment process: The heat treatment process adopts normalizing (rapid cooling) + tempering.
[0009] Furthermore, the normalizing holding temperature of the present invention is 890-910°C, the time in the furnace is the plate thickness (mm) × 2.0-2.5 (min / mm), and the plate is quickly cooled by water after being taken out of the furnace; the tempering holding temperature is 650-680°C, the time in the furnace is the plate thickness (mm) × 3.0-3.5 (min / mm), and the plate is air-cooled after being taken out of the furnace.
[0010] Furthermore, the thickness of the steel plate produced by the present invention is 100-145 mm.
[0011] Furthermore, the single value of the impact energy of the core of the steel plate produced by the present invention at -45°C is ≥100J.
[0012] Furthermore, the performance of the steel plate produced by the present invention meets the requirements of ASME SA516 / SA516M-2023 standards.
[0013] Beneficial effects of the present invention:
[0014] (1) By controlling the furnace temperature, furnace time, soaking zone temperature and time, the slab is heated evenly, the elements diffuse evenly, and overburning that causes coarse grains is avoided;
[0015] (2) The deformation of the core of the steel plate is increased through a two-stage controlled rolling process, which effectively refines the core structure of the steel plate and improves the uniformity of the core structure;
[0016] (3) Through the normalizing (rapid cooling) + tempering heat treatment process, pearlite + cementite + acicular ferrite structure is obtained, the structure is further refined, and the steel plate has excellent low-temperature toughness and strength-toughness matching;
[0017] (4) The thick SA516Gr.70 steel plate produced by the method of the present invention has a core-45°C impact energy single value of ≥100J, and the stability of the low-temperature impact toughness of the core is relatively high. Other properties meet the requirements of the ASME SA516 / SA516M-2023 standard. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0019] Figure 1 This is a 500-fold microstructure diagram of 1 / 2 the thickness of the steel plate in Example 1;
[0020] Figure 2 The typical morphology and composition diagram of inclusions in Example 1;
[0021] Figure 3 The typical morphology and composition diagram of inclusions in comparative example 1;
[0022] Figure 4 This is the metallographic structure diagram of Comparative Example 2. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Embodiment 1:
[0025] The thickness of the thick SA516Gr.70 steel plate in this embodiment is 110 mm, and the chemical composition mass percentage of the steel plate is: C: 0.15%, Si: 0.17%, Mn: 1.42%, P: 0.009%, S: 0.002%, Alt: 0.033%, Nb: 0.018%, V: 0.027%, Ni: 0.34%, Cu: 0.26%, and the others are Fe and essential residual elements.
[0026] The method for improving the low-temperature toughness of the core of a thick SA516Gr.70 steel plate described in this embodiment includes the steps of slab heating, rolling and heat treatment, and the specific process steps are as follows:
[0027] (1) Slab heating process: heating furnace hearth temperature 1222~1248℃, soaking temperature 1187~1216℃, furnace time 11h, soaking time 53min;
[0028] (2) Rolling process: the starting rolling temperature of the first stage is 1087°C, the final rolling temperature is 992°C, the reduction rates of the last three passes are 18%, 21%, and 20% respectively, and the intermediate billet thickness is 230 mm; the starting rolling temperature of the second stage is 868°C, the final rolling temperature is 784°C, and the steel is rapidly cooled by water after rolling, and the red-returning temperature is 702°C;
[0029] (3) Heat treatment process: Normalizing holding temperature is 890℃, the time in the furnace is 262min, and the steel is quickly cooled by water after being taken out of the furnace; tempering holding temperature is 680℃, the time in the furnace is 392min, and the steel is air cooled after being taken out of the furnace.
[0030] The mechanical property test results of the 110 mm thick SA516Gr.70 steel plate in this embodiment are: yield strength 386 MPa, tensile strength 535 MPa, elongation 30%, and low-temperature impact energy of -45°C at the 1 / 2 thickness position 231 J, 264 J, and 255 J.
[0031] Embodiment 2:
[0032] The thickness of the thick SA516Gr.70 steel plate in this embodiment is 125 mm, and the chemical composition mass percentage of the steel plate is: C: 0.14%, Si: 0.19%, Mn: 1.45%, P: 0.008%, S: 0.002%, Alt: 0.029%, Nb: 0.019%, V: 0.026%, Ni: 0.35%, Cu: 0.28%, and the others are Fe and essential residual elements.
[0033] The method for improving the low-temperature toughness of the core of a thick SA516Gr.70 steel plate described in this embodiment includes the following steps:
[0034] (1) Slab heating process: heating furnace hearth temperature 1218 ~ 1245 ° C, soaking temperature 1183 ~ 1214 ° C, furnace time 10 hours, soaking time 56 minutes;
[0035] (2) Rolling process: the starting rolling temperature of the first stage is 1089°C, the final rolling temperature is 989°C, the reduction rates of the last three passes are 19%, 20%, and 19% respectively, and the intermediate billet thickness is 255 mm; the starting rolling temperature of the second stage is 873°C, the final rolling temperature is 796°C, and the steel is rapidly cooled by water after rolling, and the red-returning temperature is 714°C;
[0036] (3) Heat treatment process: Normalizing holding temperature is 900℃, the time in the furnace is 284min, and rapid cooling by water after leaving the furnace; tempering holding temperature is 670℃, the time in the furnace is 403min, and air cooling after leaving the furnace.
[0037] The mechanical property test results of the 125 mm thick SA516Gr.70 steel plate in this embodiment are: yield strength 377 MPa, tensile strength 532 MPa, elongation 29%, and -45°C low-temperature impact energy 255 J, 247 J, and 231 J at the 1 / 2 thickness position.
[0038] Embodiment 3:
[0039] The thickness of the thick SA516Gr.70 steel plate in this embodiment is 140 mm, and the chemical composition mass percentage of the steel plate is: C: 0.13%, Si: 0.21%, Mn: 1.43%, P: 0.009%, S: 0.002%, Alt: 0.035%, Nb: 0.016%, V: 0.028%, Ni: 0.33%, Cu: 0.26%, and the others are Fe and essential residual elements.
[0040] The method for improving the low-temperature toughness of the core of a thick SA516Gr.70 steel plate described in this embodiment includes the following steps:
[0041] (1) Slab heating process: heating furnace hearth temperature 1215 ~ 1242 ° C, soaking temperature 1185 ~ 1216 ° C, furnace time 11h, soaking time 48min;
[0042] (2) Rolling process: the starting rolling temperature of the first stage is 1094°C, the final rolling temperature is 994°C, the reduction rates of the last three passes are 17%, 19%, and 20% respectively, and the intermediate billet thickness is 290 mm; the starting rolling temperature of the second stage is 878°C, the final rolling temperature is 801°C, and the steel is rapidly cooled by water after rolling, and the red-returning temperature is 713°C;
[0043] (3) Heat treatment process: Normalizing holding temperature is 910℃, the time in the furnace is 338min, and rapid cooling by water after being taken out of the furnace; tempering holding temperature is 650℃, the time in the furnace is 461min, and air cooling after being taken out of the furnace.
[0044] The mechanical property test results of the 140 mm thick SA516Gr.70 steel plate in this embodiment are: yield strength 371 MPa, tensile strength 524 MPa, elongation 31%, and -45°C low-temperature impact energy 226 J, 233 J, and 219 J at the 1 / 2 thickness position.
[0045] Comparative Example 1:
[0046] The thickness of the thick SA516Gr.70 steel plate of this comparative example is 108 mm, and the difference between it and Example 1 is that the chemical composition mass percentage of the steel plate is: C: 0.14%, Si: 0.19%, Mn: 1.43%, P: 0.008%, S: 0.002%, Alt: 0.029%, Nb: 0.017%, V: 0.027%, Ni: 0.32%, Cu: 0.27%, Ti: 0.016%, and the others are Fe and essential residual elements. The preparation process steps are the same as those of Example 1.
[0047] The mechanical properties test results of the 108mm thick SA516Gr.70 steel plate in this comparative example are: yield strength 372MPa, tensile strength 525MPa, elongation 30%, and low-temperature impact energy of -45°C at the 1 / 2 position of the plate thickness 47J, 36J, and 39J.
[0048] Compared with Example 1, the number of inclusions in Comparative Example 1 increased significantly, and the size increased. The proportion of inclusions of 5 μm and below decreased from 94.0% to 82.8%, and the type of inclusions changed from spherical C12A7 inclusions to sharp-angled TiN inclusions, resulting in a decrease in the low-temperature toughness of the core. The specific results are as follows Figure 2 , Figure 3 shown.
[0049] Comparative Example 2:
[0050] The thickness of the thick SA516Gr.70 steel plate in this comparative example is 112mm, and its chemical composition mass percentage is the same as that of the steel plate in Example 1, and the production method steps are roughly the same, except for the heat treatment process. Heat treatment process of comparative example 2: normalizing holding temperature is 920℃, furnace time is 254min, and water cooling is performed quickly after being taken out of the furnace; tempering holding temperature is 690℃, furnace time is 385min, and air cooling is performed after being taken out of the furnace.
[0051] The mechanical properties test results of the 112mm thick SA516Gr.70 steel plate in this comparative example are: yield strength 375MPa, tensile strength 532MPa, elongation 31%, and low-temperature impact energy of -45°C at the 1 / 2 position of the plate thickness 36J, 52J, and 47J.
[0052] Compared with Example 1, the metallographic results of Comparative Example 1 show that the lath structure is relatively coarse, and the precipitation phase segregation phenomenon is more significant, resulting in a decrease in low-temperature impact toughness. Figure 4 shown.
[0053] Comparative Example 3:
[0054] The thickness of the thick SA516Gr.70 steel plate in this comparative example is 115 mm, and its production method steps are the same as those in Example 1, except that the chemical composition mass percentages of the steel plate are: C: 0.15%, Si: 0.20%, Mn: 1.42%, P: 0.009%, S: 0.002%, Alt: 0.027%, Nb: 0.018%, V: 0.026%, Ni: 0.25%, Cu: 0.34%, and the others are Fe and essential residual elements.
[0055] The mechanical properties test results of the 115mm thick SA516Gr.70 steel plate in this comparative example are: yield strength 385MPa, tensile strength 541MPa, elongation 27%, and -45°C low-temperature impact energy 63J, 45J, and 48J at the 1 / 2 position of the plate thickness.
[0056] Compared with Example 1, Comparative Example 3 increases the Cu content and reduces the Ni content, resulting in a decrease in the toughness phase ratio, thereby reducing the core low-temperature toughness. It can be seen that the strength and toughness matching of SA516Gr.70 steel plates with large thickness can be achieved by adjusting the Ni and Cu contents.
[0057] Table 1 Properties of the steels of the embodiments of the present invention and the comparative examples
[0058]
[0059] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate, characterized in that: The chemical composition of the steel plate is as follows: C: 0.12% to 0.16%, Si: 0.15% to 0.25%, Mn: 1.40% to 1.50%, P≤0.010%, S≤0.003%, Alt: 0.020% to 0.050%, Nb: 0.015% to 0.02%, V: 0.025% to 0.030%, Ni: 0.30% to 0.40%, Cu: 0.20% to 0.30%, and the rest are Fe and essential residual elements.
2. A method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate according to claim 1, characterized in that: The method steps include: Slab heating: heating furnace hearth temperature ≤ 1250℃, soaking temperature 1180~1220℃, furnace time ≥ 10h, soaking time 40~60min; Rolling: The rolling process is divided into two stages. The starting rolling temperature of stage I is ≥1080℃, the final rolling temperature is ≥980℃, the reduction rate of the last three passes after widening is ≥17%, and the thickness of the intermediate billet is more than twice the thickness of the finished plate; the starting rolling temperature of stage II is ≤880℃, the final rolling temperature is 750~820℃, water cooling after rolling, and the red-returning temperature is 680~720℃; Heat treatment process: The heat treatment process adopts normalizing (rapid cooling) + tempering.
3. A method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate according to claim 2, characterized in that: The normalizing holding temperature is 890-910°C, the time in the furnace is plate thickness (mm) × 2.0-2.5 (min / mm), and the plate is quickly cooled by water after being taken out of the furnace; the tempering holding temperature is 650-680°C, the time in the furnace is plate thickness (mm) × 3.0-3.5 (min / mm), and the plate is air-cooled after being taken out of the furnace.
4. A method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate according to claim 3, characterized in that: The thickness of the produced steel plates is 100 to 145 mm.
5. The method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate according to claim 2, characterized in that: The single value of impact energy of the core of the produced steel plate at -45℃ is ≥100J.
6. A method for improving the low temperature toughness of the core of a thick SA516Gr.70 steel plate according to any one of claims 2 to 5, characterized in that: The performance of the produced steel plates meets the requirements of ASME SA516 / SA516M-2023 standards.
Citation Information
Patent Citations
Heavy-thickness low-temperature high-toughness A633 MOD steel plate and production method thereof
CN108486490A
Large-thickness low-temperature pressure vessel steel with good core impact toughness and manufacturing method
CN114438412A
150mm-thick FH550-grade ocean engineering steel plate with low compression ratio and excellent low-temperature toughness and preparation method of 150mm-thick FH550-grade ocean engineering steel plate
CN115074618A
Super-thick steel plate with excellent core low-temperature impact toughness and manufacturing method of super-thick steel plate
CN115094316A
Pressure vessel steel with good core impact toughness and manufacturing method thereof
CN117026108A